A facile and economical route to synthesize nano-sized ZSM-5 zeolite aggregates with mesopores was developed by a modified seed-induced method using silicate-1 (S-1) as seeds without additional templates in the presence of a trace amount of cetyltrimethylammonium bromide (CTAB). The effect of the amounts of CTAB and S-1 on the morphologies and textural properties were studied in detail, and the possible formation mechanism was proposed. The primary crystal sizes of the ZSM-5 zeolites could be adjusted and mesopores were generated in a certain range. The resulting ZSM-5 zeolites showed a uniformly conglobate morphology with particle sizes of 400–600 nm, aggregated with 20–50 nm crystallites, possessing a large external surface area and abundant inter-crystallite mesopores under the optimum synthesis conditions (CTAB to total SiO2 molar ratio was 0.02 and SiO2 in S-1 gel took up 8% to the total SiO2). The catalytic performance of nano-sized ZSM-5 zeolites in methanol to propylene reaction showed a high stability and high propylene selectivity.
To overcome these disadvantages of the pure microporosity in ZSM-5, two main strategies have been developed in recent years. One strategy is to reduce the crystal sizes of ZSM-5.9 The decrease in the crystal sizes from the micrometer to nanometer scale could increase the external surface area and decrease the diffusion path length, which is conducive for the enhancement of catalytic stability.10 Within the past few decades, nano-sized ZSM-5 zeolites have been successfully synthesized by the hydrothermal crystallization.11–13 However, zeolite crystals of particles no bigger than 100 nm might be thermodynamically unstable due to high surface energy and vast amounts of surface defects.14 Meanwhile, nanocrystals are difficult to handle and have low yields during synthesis, in which the majority of the building units are left unused in the mother liquid. Another strategy is to prepare ZSM-5 with both micropores and mesopores, which are usually referred to as mesoporous ZSM-5 or hierarchical structured ZSM-5.15 To this end, various attempts to synthesize mesopores ZSM-5 zeolites have been reported, including mainly post treatments and indirect templating methods.16 Post treatments can be divided into steaming dealumination,17–19 acid dealumination20–22 and base desilication.23–26 Though mesopores can be developed, the etching of zeolites is often accompanied by the loss of crystallinity, which leads to pernicious effects on the catalytic performance. Indirect templating method is to add a lot of meso-template agents in the synthetic gels with the micropore template of tetrapropylammonium hydroxide (TPAOH).27–30 In 2009, Choi et al.31 developed MFI zeolite nanosheets with a thickness of 2.5 nm along the b-axis by designing a di-quaternary ammonium-type surfactant, and the MFI zeolite nanosheets dramatically suppressed the catalyst deactivation through coke deposition in methanol-to-gasoline conversion. Recently, Kim et al.32 also reported that MFI zeolite nanosheets synthesized with multi ammonium surfactants showed greater activity and selectivity to propylene and longer lifetimes than commercial ZSM-5 in the MTP reaction, this was attributed to the well-developed nanosheet structure with a high specific surface area and a large mesopore volume. Zhang et al.33 developed a hierarchical ZSM-5 zeolite with b-oriented thinner dimension in fluoride medium, and the obtained material displayed a greatly longer catalytic lifetime and higher propylene selectivity in MTP reaction than conventional ZSM-5 catalysts, due to the superior diffusivity of thinner b-axis path and intracrystal secondary mesopores. However, with these methods, the large usage of TPAOH and mesoporogens makes the ZSM-5 zeolites expensive and produces environmental pollution.
A seed-induced method is an interesting alternative to synthesize the nano-sized ZSM-5 zeolites since its low consumption of templates and rapid crystallization of ZSM-5 zeolites.34,35 Nevertheless, the intergrowth and secondary growth of crystals usually occur, leading to the formation of compact aggregates with larger crystal sizes in respect to the seed particles.34 To overcome the problem, the effort has been done to develop seed-induced method in the presence of various mesoporogens such as cationic surfactants and special organosilanes. Frunz and co-workers36 reported that the mesoporous ZSM-5 crystals were synthesized by aging of ZSM-5 synthesis solution to form the protozeolitic seeds, and subsequently adding a surfactant of cetyltrimethylammonium chloride (CTACl). Nearly identical method was adopted to synthesize hierarchical mesoporous ZSM-5 using cetyltrimethylammonium bromide (CTAB) instead of CTACl by Zhu et al.14 and Gonçalves et al.37 However, in these methods, a large number of TPAOH and CTAB were still used. Recently, Gao et al.38 prepared a series of ZSM-5 nanozeolites with hierarchical porosity by a seed-assisted method and the addition of phenylaminopropyltrimethoxysilane (PATMOS) into the medial synthesis system. The molar ratio of TPAOH introduced by the addition of seeds to total SiO2 (TPAOH/SiO2) is 0.05–0.1, much lower than above methods, but the use of expensive organosilanes restricts its wide range of applications in industry.
Herein, nano-sized ZSM-5 zeolite aggregates were directly synthesized by a facile and economical approach using silicalite-1 (S-1) as seeds in the presence of CTAB. The obtained ZSM-5 zeolites display high crystallinity, large specific surface area and external surface area, abundant intercrystal mesoporosity due to self-assembled nanocrystallites and a markedly improvement in the stability and propylene selectivity in MTP reaction. Moreover, the synthesis method has the advantage of low TPAOH and CTAB consumption (TAPOH/SiO2 = 0.018, CTAB/SiO2 = 0.02).
To better investigate the effect of CTAB added in the precursor solution on the properties of the final ZSM-5 products, five samples with different CTAB/SiO2 ratios (0.005, 0.015, 0.02, 0.03 and 0.05, respectively) were synthesized with the same synthesis method of N-ZSM-5, and they were denoted as Z-xC-0.08S (x represents the CTAB/SiO2 molar ratio). Here, N-ZSM-5 (CTAB/SiO2 = 0.02) was re-synthesized in order to prove the reliability of this synthesis method, and denoted as Z-0.02C-0.08S. For comparison, conventional ZSM-5 (denoted as Con-ZSM-5) was synthesized under the same condition of N-ZSM-5, but in the absence of CTAB. Both representative N-ZSM-5 and Con-ZSM-5 zeolites were ion exchanged three times in 1 M NH4NO3 solution at 80 °C for 2 h, and then calcined at 550 °C to obtain the H-type ZSM-5.
Similarly, to investigate the effect of seeds on the properties of ZSM-5 zeolites, four samples with different S-1/SiO2 ratios (0.005, 0.02, 0.04 and 0.06, respectively) were synthesized with the same synthesis method of N-ZSM-5, and they were denoted as Z-2C-yS (y represents the S-1/SiO2 ratio).
X-ray diffraction (XRD) patterns were obtained at room temperature on a Rigaku D/max 2500 diffractometer employing the graphite filtered Cu Kα radiation (λ = 0.1542 nm) with a scanning rate of 8° min−1 in the 2θ ranges from 5° to 55°.
Nitrogen adsorption and desorption isotherms of the samples were measured at liquid N2 temperature (77 K) on a Micromeritics TriStar 3000 automated physisorption instrument. Prior to the measurements, all the samples were degassed at 300 °C for 4 h. The total specific surface area (SBET) was derived from the Brunauer–Emmett–Teller (BET) equation. The micropore surface area (Smicro) was derived from the t-plot method, and external surface area (Sext) was calculated by subtracting Smicro from SBET. The total pore volume (Vtotal) was calculated at p/p0 = 0.99. The micropore volume (Vmicro) was also derived from the t-plot method, and mesopore volume (Vmeso) was calculated by subtracting Vmicro from Vtotal. The mesopore size distributions were estimated by using the Barrett–Joyner–Halenda (BJH) method from the desorption branch of the isotherms.
Fourier transform infrared (FT-IR) spectra of the samples were recorded in a Bruker Vertex 7.0 spectrometer, using the KBr wafer technique. The infrared absorbance spectra were recorded from 2000 to 400 cm−1 with a resolution of 4 cm−1.
Temperature-programmed desorption of ammonia (NH3-TPD) measurements were recorded using a Micromeritics 2910 chemical adsorption instrument. The samples were pretreated in a nitrogen flow at 400 °C for 1 h, and then cooled down to 100 °C, and ammonia was introduced with nitrogen as the carrier gas. After 60 min, the flow was switched to nitrogen, and the sample was heated to 700 °C at a rate of 10 °C min−1. The desorbed ammonia was monitored by a thermal conductivity detector.
Solid-state magic angle spinning nuclear magnetic resonance (MAS NMR) was used to investigate the coordination of Al and Si atoms in the ZSM-5 framework. The measurements were performed on a Varian infinityplus 300 MHz NMR spectrometer equipped with two radio frequency channels at a field strength of 7.0 T. 27Al MAS NMR spectra were recorded at 104.2 MHz at a spinning frequency of 5 kHz and 2.05 s intervals between successive accumulations. 29Si MAS NMR spectra were recorded at 79.4 MHz at a spinning frequency of 5 kHz and 6.05 s intervals between successive accumulations.
Elemental analyses were carried out on an inductively coupled plasma optical emission spectroscope (ICP-OES) using a Varian Vista-MPX emission spectrometer.
Thermogravimetric (TG) analysis was evaluated by Shimadzu TGA-50 apparatus using a temperature ramp from 30 to 800 °C with a heating rate of 10 °C min−1 in oxygen atmosphere.
(1) |
(2) |
Samples | CTAB/SiO2 ratio | S-1/SiO2 ratio | SiO2/Al2O3 ratioa | SBETb (m2 g−1) | Smicroc (m2 g−1) | Sextc (m2 g−1) | Vtotald (cm3 g−1) | Vmicroe (cm3 g−1) | Vmesoe (cm3 g−1) |
---|---|---|---|---|---|---|---|---|---|
a Determined by ICP-OES.b Derived from the BET equation.c Micropore surface area (Smicro) was derived from the t-plot method, Sext was calculated by subtracting Smicro from SBET.d Calculated at p/p0 = 0.99.e Micropore volume (Vmicro) was evaluated by the t-plot method, Vmeso was calculated by subtracting Vmicro from Vtotal. | |||||||||
N-ZSM-5 | 0.02 | 0.08 | 157 | 414 | 141 | 273 | 0.31 | 0.08 | 0.23 |
Con-ZSM-5 | 0 | 0.08 | 155 | 342 | 181 | 161 | 0.21 | 0.12 | 0.09 |
Z-0.005C-0.08S | 0.005 | 0.08 | 146 | 366 | 174 | 192 | 0.22 | 0.10 | 0.12 |
Z-0.015C-0.08S | 0.015 | 0.08 | 152 | 388 | 169 | 219 | 0.24 | 0.08 | 0.16 |
Z-0.02C-0.08S | 0.02 | 0.08 | 158 | 416 | 145 | 271 | 0.30 | 0.07 | 0.23 |
Z-0.03C-0.08S | 0.03 | 0.08 | 151 | 358 | 154 | 204 | 0.22 | 0.07 | 0.15 |
Z-0.05C-0.08S | 0.05 | 0.08 | 157 | 318 | 169 | 149 | 0.17 | 0.10 | 0.07 |
Z-0.02C-0.005S | 0.02 | 0.005 | 152 | 323 | 171 | 152 | 0.19 | 0.07 | 0.12 |
Z-0.02C-0.02S | 0.02 | 0.02 | 147 | 369 | 192 | 177 | 0.23 | 0.09 | 0.14 |
Z-0.02C-0.04S | 0.02 | 0.04 | 155 | 373 | 173 | 200 | 0.26 | 0.09 | 0.17 |
Z-0.02C-0.06S | 0.02 | 0.06 | 159 | 381 | 168 | 213 | 0.26 | 0.07 | 0.19 |
XRD patterns (Fig. 2a) show that N-ZSM-5 has a typical MFI structure (peaks at 2θ of 7.9°, 8.7°, 23.1°, 23.9° and 24.4°).39 FT-IR spectra (Fig. 2b) of N-ZSM-5 show intensive absorption bands at 1150–1050 cm−1, 795 cm−1 and 455 cm−1, associated with internal asymmetric stretch, external symmetric stretch and T–O bend respectively.7 The optical density ratios of the absorption bands at 550 cm−1 and 455 cm−1 for N-ZSM-5 is 0.71, which is near to 0.7 for pure pentasil samples with high crystallinity of ZSM-5,7 indicating that N-ZSM-5 has a good MFI frame structure.
Fig. 2 XRD patterns (a), FT-IR spectra (b), 27Al MAS NMR spectra (c) and 29Si MAS NMR spectra (d) of N-ZSM-5. |
27Al and 29Si MAS NMR was used to further reveal the coordination of Al and Si atoms in N-ZSM-5. One distinctive resonance peak at a chemical shift of 53 ppm in the 27Al MAS NMR spectrum (Fig. 2c) which corresponds to tetrahedrally coordinated Al in the zeolite framework is observed. Moreover, no resonance at 0 ppm, typically associated with the octahedrally coordinated Al in the extra-framework positions,41 confirms that the Al atoms are totally incorporated into the crystal frameworks of the N-ZSM-5. Fig. 2d shows the 29Si MAS NMR spectra of N-ZSM-5. The intensive resonances at 114.5 ppm and 111.0 ppm are associated to the Si (4Si, 0Al) sites, and the peak at 104.2 ppm corresponds to Si (3Si, 1Al) sites.42 Resonances representing Si (2Si, 2Al) with chemical shift below 100 ppm sites are not observed, indicating that [Al–O–Si–O–Al] sequences are not present in the highly siliceous N-ZSM-5.43 The resonance at 100.7 ppm of N-ZSM-5 belongs to the Si (3Si, 1OH) sites, which can be attributed to the hydroxyl groups on the large external surface of N-ZSM-5.28
The XRD patterns (Fig. 3) of all the synthesized samples show typical diffraction characteristics for ZSM-5 structure, and no amorphous phase is detected, suggesting that they are successfully synthesized. The corresponding SEM images of the samples with different CTAB/SiO2 ratios are shown in Fig. 4. Though all the samples have similar particle sizes, their morphologies are distinctly different. Con-ZSM-5 (Fig. 4a) has irregular block-like morphology aggregated with nanocrystals above 100 nm sizes. After the addition of CTAB, the morphologies of the samples (Fig. 4b–f) show significant change compared to that of Con-ZSM-5. At the relatively low CTAB/SiO2 ratio from 0.005 to 0.02, the particles of ZSM-5 zeolites comprise the globular agglomerates of nano-crystallites, and the average sizes of the nano-crystallites gradually decrease to 30 nm, which is much smaller than that of Con-ZSM-5. The results indicate that CTAB may interact with the crystal nucleus and inhibit the crystal growth. The SEM image (Fig. 4d) of the sample with CTAB/SiO2 ratio of 0.02 is in good accordance with that of the N-ZSM-5 (Fig. 1b), confirming the repeatability of this method to synthesize nano-sized ZSM-5 aggregates with mesopores. While the samples with CTAB/SiO2 ratio of 0.03 and 0.05 (Fig. 4e and f) show less rough surface, indicating that excessive amounts of CTAB results in the growth of crystal again.
Fig. 3 XRD patterns of Con-ZSM-5 and ZSM-5 zeolites synthesized with different CTAB/SiO2 ratios: 0.005, 0.015, 0.02, 0.03 and 0.05. |
Fig. 4 SEM images of Con-ZSM-5 (a), and ZSM-5 zeolites synthesized with different CTAB/SiO2 ratios: (b) 0.005, (c) 0.015, (d) 0.02, (e) 0.03 and (f) 0.05. All scale bars are 1 μm. |
To clarify the behaviour of CTA+ in the synthesis, it is useful to evaluate the amount of CTA+ incorporated in the as-synthesized samples by TG analysis. Fig. 5a presents the TG curves of Con-ZSM-5 and N-ZSM-5 synthesized with different CTA+/SiO2 ratio before calcination. All samples show two regions of weight loss. The first region below 300 °C is assigned to desorption of water. Both Con-ZSM-5 and the sample with CTAB/SiO2 ratio of 0.005 have a weight loss of 1.3%. Increasing the CTAB/SiO2 ratio to 0.5, the weight loss increases greatly to 6.8%. This may be ascribed to hydrophilicity of the surface with more CTAB, which adsorbs more water. The second region of 300–500 °C is ascribed to the combustion of the organic template.44 For Con-ZSM-5, the organic template of TPAOH is introduced in trace amount (TPA+/SiO2 = 0.018) with the S-1 seeds, but the weight loss is 7.4%, which is much larger than the mass percentage of TPA+ in the total mass (2.2%). Therefore, it is believed that the more weight loss is attributed to the condensation water from the elimination of the surface hydroxyl groups or removal of chemically bound water.45 For N-ZSM-5 with CTAB/SiO2 of 0.005, the weight loss increases by 1.8% in comparison with that of Con-ZSM-5, proving that most of CTA+ is occluded into the as-synthesized sample. However, when more CTAB is added, i.e., with CTAB/SiO2 of 0.02 and 0.05, the weight loss only increases slightly, indicating that the excessive amounts of CTAB cannot be occluded into the as-synthesis samples. Fig. 5b further shows the amount of CTA+ incorporated into the samples and the variation of mesopore volumes as a function of CTA+/SiO2 ratios. With the addition of CTAB at low level, the mesopore volume increases due to the incorporation of CTA+ into the samples and/or the interaction of CTA+ with the crystal nucleus to restrain the growth of crystals and form nano-sized aggregates. However, the addition of excessive amounts of CTAB is not needed and has a negative effect with the mesopore volume being decreased.
XRD patterns in Fig. 6 show that all the synthesized samples with high crystallinity are obtained. SEM images of ZSM-5 zeolites synthesized with different S-1/SiO2 ratios are shown in Fig. 7. All the ZSM-5 zeolites are the aggregated spheres of nano-crystallites. Although the average particle sizes of ZSM-5 zeolites have a reduction from 800 nm to 500 nm with increasing the S-1/SiO2 ratio of 0.005 to 0.02, all the ZSM-5 zeolites show almost same average particle sizes around 500 nm further increasing the S-1/SiO2 ratio up to 0.06. It should be pointed out that the average sizes of primary nano-crystallites gradually decrease from 100 nm to 40 nm with the increase of the S-1/SiO2 ratio, which conduces to the increase of SBET, Sext, Vtotal and Vmeso, as shown in Table 1. Similar results are also reported by Teng et al., who believed that more nuclei and surface were provided with the increase of seeds, and accordingly the primary particle became smaller.35 The result of SEM images reveals that the employed amount of seeds has an important effect not only on the size of the ZSM-5 zeolites particles but also on the primary nano-crystallites.
Fig. 6 XRD patterns of ZSM-5 zeolites synthesized with different S-1/SiO2 ratios: 0.005, 0.02, 0.04 and 0.06. |
Fig. 7 SEM images of ZSM-5 zeolites synthesized with different S-1/SiO2 ratios: (a) 0.005, (b) 0.02, (c) 0.04 and (d) 0.06. All scale bars are 1 μm. |
Fig. 8 SEM image of S-1 seed (a) and proposed mechanism for the synthesis of nano-sized ZSM-5 aggregates by modified seed-induced method with CTAB (b). |
Catalysts | Total acidity/(mmol g−1) | Strong acidity/(mmol g−1) | Weak acidity/(mmol g−1) |
---|---|---|---|
N-ZSM-5 | 0.314 | 0.149 | 0.165 |
Con-ZSM-5 | 0.290 | 0.140 | 0.150 |
To quickly evaluate the catalytic activities, MTP reactions over N-ZSM-5, Con-ZSM-5 and commercial ZSM-5 were carried out with WHSV of 8 h−1. The conversion of methanol is presented as a function of time on stream (TOS) for the three catalysts in Fig. 10a. Methanol conversions over N-ZSM-5, Con-ZSM-5 and commercial ZSM-5 are approximately 100% during the initial 37 h, 11 h and 20 h TOS, respectively, indicating the high initial stability of all catalysts. If the catalyst deactivation is defined as methanol conversions decreasing to around 95%, the catalytic lifetime of N-ZSM-5 (40 h) is much longer than that of Con-ZSM-5 (15 h) and commercial ZSM-5 (25 h). Therefore, compared with Con-ZSM-5 and commercial ZSM-5, N-ZSM-5 exhibits a pronounced improvement of the stability.
Fig. 10b displays the selectivity of propylene over N-ZSM-5, Con-ZSM-5 and commercial ZSM-5 catalysts as a function of TOS. At the initial stage (0.3 h), the selectivity towards propylene is amount to 38.6% for N-ZSM-5, remarkably higher than that of Con-ZSM-5 (32.2%) and commercial ZSM-5 (37.4%). The steady state with the stable propylene selectivity of the reaction is observed after about 2 h TOS for N-ZSM-5, 5 h for Con-ZSM-5 and 8 h for commercial ZSM-5. The steady period of reaction for N-ZSM-5 reaches more than 30 h, much longer than Con-ZSM-5 (13 h) and commercial ZSM-5 (18 h). The selectivity of ethylene and light olefin (C2–C4) for N-ZSM-5, Con-ZSM-5 and commercial ZSM-5 are shown in Fig. 10c and d. The average values of selectivity towards propylene, ethylene and C2–C4 for N-ZSM-5 at steady state are 39.5%, 12.2% and 71.7%, respectively, higher than Con-ZSM-5 (35.7%, 10.6% and 62.3%, respectively) and commercial ZSM-5 (37.9%, 11.5% and 67.9%, respectively), leading to a similar propylene/ethylene ratio (3.23, 3.36 and 3.29 respectively). With prolonged TOS, the deactivation stage occurs, and the propylene selectivity for all catalysts decreases slowly.
Fig. 11 further shows the coke deposition on the deactivated N-ZSM-5 and Con-ZSM-5 catalysts measured by TG analysis. N-ZSM-5 contains 2.43 wt% coke deposit after 41 h TOS, while for Con-ZSM-5 the coke deposit is 2.11 wt% after 16 h. The average coking rate on N-ZSM-5 is 0.06% per hour, much lower than that of 0.13% on Con-ZSM-5 catalyst. N-ZSM-5 exhibits a strong capability for coke tolerance, and retardation of catalyst deactivation. The excellently catalytic performance of N-ZSM-5 catalyst owes to that the nano sizes, large external surface area, and abundant mesopores of N-ZSM-5 can improve the diffusivity of methanol and products, and restrain the coke deposition,48 thereby leading to the pronounced improvement of catalytic stability and propylene selectivity in MTP reaction.
This journal is © The Royal Society of Chemistry 2016 |