Tetragonal La2(MoO4)3 with various novel and complex 3D hierarchical architectures self-assembled from different building blocks were successfully synthesized by a hydrothermal method in EDTA-mediated processes. X-ray diffraction (XRD), scanning electron microscopy (SEM), transmission electron microscopy (TEM) and high resolution transmission electron microscopy (HRTEM) were employed to characterize the as-obtained products. It was found that morphology modulation could be easily realized simply by changing the amount of EDTA introduced into the reaction system. The amount of EDTA not only affected the substructures of the hierarchical structures, but also determined the size distributions of the final products. The formation mechanisms for different hierarchical architectures were proposed on the basis of a series of time-dependent experiments. An investigation on the photoluminescence (PL) properties of La2(MoO4)3:Eu with different morphologies revealed that the optical properties were strongly correlated with the morphology and size. Furthermore, as highlighted by the fascinating hierarchical structures of La2(MoO4)3, the potential application of La2(MoO4)3 as an absorbent in water treatment was also investigated for the first time. Possible reasons responsible for the differences in photoluminescence behaviors and absorption activities of different hierarchical architectures were discussed.
Rare earth molybdate compounds, R2(MoO4)3 and R2MoO6 (R = rare earth elements), have attracted extensive attention because of their potential technological applications as catalysts, high-performance phosphors, up-conversion materials, negative thermal expansion materials and so forth.12–15 Nevertheless, most of the previous works about rare earth molybdate compounds are mainly concentrated on the bulk materials obtained by conventional solid-state reaction, and little has been done on the fabrication of 3D hierarchical structures. Recently, several 3D La2(MoO4)3 microarchitectures obtained in the presence or absence of different kinds of surfactants have been reported.16 Nevertheless, to the best of our knowledge, up till now there is no systematic study on the shape control of 3D La2(MoO4)3 superstructures, especially hierarchical structures constructed by different building blocks.
Herein, for the first time we report an efficient method for the controlled fabrication of several different and novel hierarchical architectures of La2(MoO4)3 with a high yield and good uniformity via a facile and mild hydrothermal route in EDTA-mediated processes. The effects of the amount of EDTA introduced into the reaction systems and the pH value of the precursor solution on the product morphology were discussed in detail. The possible formation mechanisms of different hierarchical superstructures were put forward on the basis of a series of time-dependent experiments. To evaluate the potential applications of our products, the photoluminescent (PL) properties of the Eu-doped La2(MoO4)3 superstructures with different morphologies were measured. Furthermore, as highlighted by the fascinating hierarchical structures of La2(MoO4)3, the adsorption activities of La2(MoO4)3 as an absorbent in water treatment were also tested. The intensive relationship between microstructure and the property of the obtained products was discussed.
The phase purity and crystallinity of the products were identified by XRD on a Philip-X'Pert X-ray diffractometer equipped with a Cu-Kα radiation source (λ = 1.540562 Å) at a scanning rate of 0.02° s−1 in a 2θ range of 10–80°. The product morphology was investigated by scanning electron microscopy (SEM JEOL JEM-6300F) and transmission electron microscopy (TEM JEOL JEM-200CX, operated at an accelerating voltage of 200 kV). For TEM observation, the samples were dispersed in ethanol by ultrasonic treatment and dropped on carbon-copper grids. The nitrogen adsorption-desorption isotherms were measured on an ASAP 2020 apparatus at liquid nitrogen temperature. PL excitation and emission spectra were recorded on an Aminco Bowman luminescence spectrometer at room temperature.
The absorption activities of the La2(MoO4)3 samples with different morphologies were evaluated via the adsorption of Rhodamine B (Rh B) dye in an aqueous solution at ambient temperature. A beaker with capacity ca. 100 mL was used as the reaction vessel. 10 mg of the samples was added to the Rh B solution (10 mg L−1, 50 mL) under stirring. UV-vis absorption spectra were recorded at different time intervals to monitor the process.
Fig. 1 XRD patterns of the as-synthesized products obtained at pH = 9 in the presence of different amounts of EDTA. (a) 0.05 g EDTA. (b) 0.10 g EDTA. (c) 0.15 g EDTA. (d) 0.25 g EDTA. (e) 0.46 g EDTA. |
Fig. 2 SEM images of the La2(MoO4)3 hierarchical microflowers obtained in the presence of 0.05 g EDTA at pH = 9. (a) Panoramic image; (b) magnified image; (c) image of an individual hierarchical microflower with 3 levels of structures; (d) high-magnification SEM image of the marked part in panel c. |
Fig. 3 SEM images of the La2(MoO4)3 microspheres built from different subunits obtained at pH = 9 with different amounts of EDTA. (a)–(c) 0.10 g EDTA. (d)–(f) 0.15 g EDTA. (g)–(i) 0.46 g EDTA. |
Besides the amount of EDTA introduced into the reaction system, the pH value of the precursor solution also had a significant influence on the product morphology. As shown in Fig. 4a and 4b, when the amount of EDTA was 0.35 g and the pH value was adjusted to 7, the product appeared as spindle-like microstructures with an average length of 2.2 μm and width of 900 nm, respectively. The micro-spindles are consisted of numerous nanoparticles with a mean size of 50 nm. When the pH value was increased to 9, the product was totally composed of microspheres with a diameter of ∼2.1 μm (Fig. 4c). A close look revealed that these microspheres with coarse surfaces were entirely constructed by nanoparticles (Fig. 4d). A further increase of pH value to 10 led to the formation of micro-flowers with an average size of 1.9 μm (Fig. 4e) and each microflower was constructed from nanoflakes with a thickness around 40 nm (Fig. 4f). The nanoflakes extended outwards from the center of the flower and were linked together through edge-to-edge and edge-to-surface conjunctions. As displayed in Fig. 4g, when the amount EDTA was 0.50 g and the pH value was 7, the as-obtained product was in the form of dumbbells with an average size of 5.0 μm. The high-magnification SEM image in Fig. 4h provides the detailed configuration of the dumbbells. The dumbbells are built from a large number of highly oriented nanoparticles and the dual fantails with rough surface take on a cauliflower-like appearance and are about 4.0 μm in diameter. Therefore, on the basis of the aforementioned SEM results, the amount of EDTA not only affects the product morphology, but also determines the size of product. By changing the amount of EDTA and the pH value, various self-assembled 3D La2(MoO4)3 hierarchical architectures such as microflowers, microspheres, microspindles and microdumbbells can be obtained and the building blocks of different hierarchical architectures vary from 3D dendrites to 2D nanoplates and eventually to 0D nanoparticles. Moreover, the greater the amount of EDTA, the smaller the average size of product. A brief summary of the detailed experimental conditions and the corresponding product morphologies is listed in Table 1.
Fig. 4 SEM images of the products obtained at different pH values with appropriate amount of EDTA. (a)–(b) pH = 7, 0.35 g EDTA. (c)–(d) pH = 9, 0.35 g EDTA. (e)–(f) pH = 10, 0.35 g EDTA. (g)–(h) pH = 7, 0.50 g EDTA. |
Sample | pH value | Amount of EDTA/g | Average size/μm | Morphology |
---|---|---|---|---|
S1 | 9 | 0.05 | 7.5 | Microflowers assembled by hyperbranched 3D dendrites |
S2 | 9 | 0.10 | 4.8 | Microflowers assembled by 2D nanoflakes |
S3 | 9 | 0.15 | 4.1 | Mixture of microspheres constructed by 2D nanoflakes and 0D nanoparticles, respectively |
S4 | 9 | 0.35 | 2.1 | Microspheres constructed by 0D nanoparticles |
S5 | 9 | 0.46 | 1.2 | Microspheres constructed by 0D nanoparticles |
S6 | 7 | 0.35 | 2.2 | Microspindles constructed by 0D nanoparticles |
S7 | 10 | 0.35 | 1.9 | Microflowers built from 2D nanoflakes |
S8 | 7 | 0.5 | 5.0 | Microdumbbells with two cauliflower-like fantails constructed by 0D nanoparticles |
More details about the morphological and structural features were further investigated by employing TEM and HRTEM. Fig. 5a presents the representative TEM image of the La2(MoO4)3 microflowers obtained with the assistance of 0.05 g EDTA. It confirms that La2(MoO4)3 spherical architectures have an average diameter about 7.5 μm, which is consistent with the above SEM observation (Fig. 2a). The as-obtained La2(MoO4)3 superstructures were stable enough to withstand ultrasonic treatment for 30 min. They preserved their integrity and only some irregular nanoflakes were peeled from the flowers (Fig. 5b), indicating that strong chemical bonding existed between the building blocks. Fig. 5c displays the HRTEM image of the nanoflake performed on the marked area in Fig. 5b, the single-crystalline nature and the particular orientation of the nanoflake are clearly demonstrated and clarified. The interplanar lattice spacing was determined to be 0.329 nm, corresponding to (112) planes of La2(MoO4)3. The corresponding SAED pattern (the inset in Fig. 5c) further confirms the single-crystalline nature of the isolated nanoflake. Fig. 5d shows the typical TEM image of the microspheres obtained in the presence of 0.35 g EDTA. The uniform microspheres with obvious rough surfaces have an average diameter of 2.1 μm, which is in good accordance with the SEM image shown in Fig. 4d. The ED pattern recorded on an individual microsphere is inset in Fig. 5d, demonstrating the polycrystalline nature of the hierarchical structure. However, the symmetrical spot pattern also indicates that the hierarchical structure is built from single-crystalline building blocks. HRTEM image taken from the fringe of a microsphere marked by the red circle in Fig. 5e is shown in Fig. 5f. From the image, the lattice interplanar spacing was determined to be 0.332 nm, corresponding to the (112) planes of La2(MoO4)3. This result also confirms the single-crystalline nature of the nanoparticles. The EDX spectrum (Fig. 5g) was employed to determine the chemical composition of the as-obtained products. The result reveals that the product only consists of La, Mo, and O. The corresponding atomic ratio of is 1:1.47:7.40, which is very close to the stoichiometric proportion of La2(MoO4)3.
Fig. 5 (a) TEM image of the microflowers obtained with the assistance of 0.05 g EDTA. (b) TEM image of the irregular nanoflakes peeled from integrated flowers after ultrasonic treatment for 30 min. (c) HRTEM image and ED pattern of a single nanoflake. (d) Representative TEM image of the microspheres obtained in the presence of 0.35 g EDTA (inset: ED pattern of an individual microsphere). (e) TEM image of the fringe of an individual microsphere. (f) HRTEM image of a nanoparticle marked in (e). (g) EDS spectrum of the microspheres. |
Concerning the thermal stability of the as-obtained products with different morphologies, a series of experiments were carried out to investigate the effect of calcination temperature on the crystallinity and morphology of the products. Three different hierarchical structures (S1, S2 and S5) were calcined at 350, 500, 650 and 800 °C in air for 3h, respectively. The crystallinity and morphology of the calcined products were characterized by XRD and SEM techniques.
Fig. SI1 in the Supporting Information† shows the XRD patterns of S1 calcined at different temperatures. It is evident that the product crystallinity is improved, as expected, with the increase of calcination temperature. Therefore, the calcined products exhibit higher diffraction intensity and narrower peaks due to the enhancement of crystallization. However, when the calcination temperature is increased to 800 °C, a second phase assigned to La2Mo2O9 (JCPDS 23-1145) can be occasionally detected to a certain extent, as marked by asterisks in Fig. SI1. Likewise, such a tendency is also observed for S2 and S5 (see Fig. SI2 and SI3), namely, the higher the calcination temperature, the higher the product crystallinity, and the impurity phase of La2Mo2O9 appears when the calcination temperature is raised to 800 °C.
Fig. SI4 displays a series of SEM images of S1 after calcination at different temperatures. It can be concluded that the hierarchical microstructures experience a great change upon calcination, although the external shape is almost maintained. It is noteworthy that the hierarchical microstructures can be successfully sustained and the characteristic morphology of the dendrites remains unchanged when the calcination temperature is below 500 °C, indicating that a rather high activation energy is needed for the collapse of these hierarchical structures (Fig. SI4a–d). As depicted in Fig. SI4e–f, the nanoflakes begin to fuse with each other after calcination at 650 °C for 3h, yet the main trunks of the dendritic structures still exist. However, when the calcination temperature is further increased to 800 °C, the characteristic morphology of dendrites no longer exists. Under this high-temperature condition, the relatively high surface energies of nanoflakes and main trunks cause the dendritic structures to further melt into each other, giving rise to the honeycomb-like structures made of numerous highly cross-linked nanoparticles (Fig. SI4g–h).
Similarly, S2 and S5 can also preserve their original morphology when the calcination temperature is below 500 °C (see Fig. SI5a–d and Fig. SI6a–b, respectively). Nevertheless, after calcination at 650 and 800 °C, respectively, the nanoflakes of S2 are fused with each other to different extents and evolve into a great many cross-linked nanoparticles, bringing out porous microspheres with different pore sizes (Fig. SI5e–h). However, the nanoparticles on the surface of the microspheres in S5 melt into each other to form bigger particles and the size of the microspheres is slightly shrunk compared with those calcined below 500 °C (Fig. SI6c–d).
Fig. 6 A series of EM images of the products collected at different reaction time intervals in the presence of 0.05 g EDTA and a pH value of 9. (a) Before hydrothermal treatment, and after hydrothermal treatment for (b) 45 min, (c) 100 min, (d) 150 min, and (e) 6 h. |
The representative SEM images of the intermediate products obtained with the assistance of 0.10 g EDTA are presented in Fig. 7. As shown in Fig. 7a, the precursor is composed of irregular nanoparticles with a size about 30 nm. After hydrothermal treatment for 20 min, these nanoparticles aggregated together to form loose spherical aggregates with a rough surface and a diameter of ∼4 μm (Fig. 7b). When the reaction time was increased to 40 min, the spherical aggregates were still the dominant structure, but some nanoplates germinating on the surface of the microsphere (marked by a red rectangle in Fig. 7c) could be occasionally observed. The inset part in Fig. 7c reveals that the nanoplates with a thickness of ∼30 nm are perpendicular to the surface and interwoven with each other. Prolonging the reaction time to 1 h gave rise to more and more nanoplates sprouted from the microsphere (see red arrowheads in Fig. 7d). As a result of continuous growth, development and ripening, numerous 2D nanoplates grew from the microsphere and were arranged in a radical direction and eventually when the reaction was allowed to proceed to 4 h the La2(MoO4)3 microspheres with flower-like appearance were formed (Fig. 7e). Based on the above SEM observation, the possible formation mechanism of the flower-like La2(MoO4)3 hierarchical hyperstructures obtained in the presence of 0.10 g EDTA can be put forward as follows. At the beginning, La3+ and EDTA form stable La3+-EDTA complex, and the addition of molybdate leads to the competition of MoO42− for La3+ with EDTA to yield La2(MoO4)3 nanoparticles. With the aid of EDTA, the incipient nanoparticles tend to self-aggregate into large microspheres mediated by hydrogen bonds. The driving force for spontaneous self-aggregation is the elimination of high energy surfaces which will lead to the substantial minimization of the surface energy from the thermodynamic viewpoint.20 On the surface-roughened microspheres, there are numerous small protuberances, which provide many high energy sites for nanocrystal growth.21 With a further increase in reaction time, the small nanoparticles would dissolve and recrystallize on the protuberances spontaneously. Furthermore, owing to the intrinsic anisotropic feature of the product, these nanocrystals prefer to grow into 2D nanoplates, such a tendency has also been reported in the previous work.16a Therefore, as the reaction continues, more and more 2D nanoplates are germinated and developed from the surface-roughened microspheres, the spherical microparticles are gradually changed to spherical flower-like architectures. The smooth surface of the nanoplates is caused by Ostwald ripening.22 Herein, the formation process of the spherical flower-like architectures can be rationally expressed as a nucleation-dissolution-recrystallization growth mechanism.
Fig. 7 A series of SEM images of the products collected at different reaction time intervals in the presence of 0.10 g EDTA and a pH value of 9. (a) Before hydrothermal treatment, and after hydrothermal treatment for (b) 20 min, (c) 40 min, (d) 1h, and (e) 4 h. |
To reveal the growth process of La2(MoO4)3 microspheres constructed by nanoparticles in the presence of 0.46 g EDTA, the products were collected at different stages and their morphologies were then investigated by TEM. As displayed in Fig. 8a, the product was composed of amorphous nanoparticles without a discernable morphology when the precursor was treated for 5 min. As the reaction was prolonged to 15 min, it could be observed that some nanoparticles were organized into spherical aggregates (marked by red circle in Fig. 8b). As the reaction went on, more and more well-defined microspheres were generated though some nanoparticles still existed in the product (Fig. 8c). Eventually, when the reaction time was further extended to more than 3 h, the remaining nanoparticles disappeared and the product was entirely composed of uniform microspheres with an average diameter of 1.2 μm (Fig. 8d). On the basis of time-dependent morphological evolution, the growth mechanism of the La2(MoO4)3 microspheres constructed by nanoparticles can be illustrated as follows. First, the introduction of molybdate into the La3+-EDTA complex led to the formation of La2(MoO4)3 nanoparticles by the competition of MoO42− for La3+ with EDTA. The strong adsorption of released EDTA on the surface of La2(MoO4)3 nuclei prevented the growth of the fresh nanoparticles. Then, the primary nanoparticles self-aggregated together to form larger microspheres mediated by hydrogen bonds and thus minimize the interfacial energy. The EDTA here can be considered as a “cohesive agent”. The continuous self-aggregation accompanying with Ostwald ripening resulted in the formation of uniform microspheres built from numerous nanoparticles. Therefore, the formation of uniform La2(MoO4)3 microspheres here can be attributed to the self-aggregation and Ostwald ripening of nanoparticles.23
Fig. 8 TEM images of the products collected at different reaction times with the aid of 0.46 g EDTA. (a) 5 min, (b) 15 min, (c) 1 h and (d) 3h. |
Concerning the three reactions carried out in the presence of different amounts of EDTA, it can be concluded that the amount of EDTA is indispensable for the morphological modulation of the final products. Introducing appropriate amounts of EDTA could prominently change the growth pathway. As mentioned above, EDTA always acts as an efficient chelating agent and capping agent to tune the product morphology. In the current study, with the increase of the amount of EDTA, the capping ability of EDTA became more and more prevailing. Therefore, when the amount of EDTA was very small, the capping ability of EDTA was negligible and the anisotropic characteristic of La2(MoO4)3 was advantageous to the generation of 2D nanoflakes as primary building blocks. However, as the amount of EDTA reached a certain value, the capping ability of EDTA was dominant, thus preventing the further growth of nuclei. Meanwhile, hydrogen bonds also played an important role in self-assembling, which was helpful to the formation of 3D hierarchical architectures. The geometrical shapes of building blocks are responsible for the generation of spherical structures, since no surfactant or emulsion was introduced during the synthesis.24 With respect to the formation of microspindles, microdumbbells and microflowers at different pH values, the pH value of the precursor solution should also have played an important role. Generally, as the pH value is reduced from 9 to 7, the selective adsorption of EDTA onto different surfaces of growing La2(MoO4)3 crystallites changes significantly, leading to dramatic modification in the final product morphologies. When the pH value was adjusted to 7, the released EDTA might be preferentially adsorbed on the lateral side of the La2(MoO4)3 crystallites, thus the longitudinal growth direction was favored. In addition, as mediated by the hydrogen bond and electrostatic effects of EDTA, the initially formed nanoparticles tended to attach with each other in a parallel way and eventually self-organized into microspindles or microdumbbells. On the other hand, when the pH value of the initial solution was increased to 10, the presence of an excess amount of OH− and NH4+ adsorbed on the surfaces of the La2(MoO4)3 crystallites led to the linkage of nanoflakes through self-assembly by electrostatic attractions and repulsions, giving rise to the appearance of flower-like architectures.5a,16a Certainly, the actual formation processes are more complex and may still remain mysterious. However, it is understandable that the intrinsic structures of La2(MoO4)3 and the external factors (such as the amount of EDTA and the pH value of the precursor solution) have synergistic effects on the formation of different hierarchical structures. The possible formation mechanisms of La2(MoO4)3 3D hierarchical architectures with different shapes obtained under different experimental conditions are schematically illustrated in Scheme 1.
Scheme 1 Schematic illustration of the morphological evolution processes of different hierarchical architectures obtained in the presence of different amounts of EDTA at pH = 9. |
Fig. 9 Room-temperature (a) excitation (λem = 614 nm) and (b) emission (λex = 396 nm) spectra of La2(MoO4)3:Eu microflowers with an average size of 7.5 μm (S1) and microspheres with an average size of 1.2 μm (S5). |
It is widely accepted that the luminescence properties of phosphors are strongly correlated with the morphology, size and crystallinity.27 In the present work, under identical measurement conditions, the relative emission intensities of the two samples are quite different, namely, the microspheres (S5) exhibit a much stronger emission than microflowers (S1). The relative intensity of the S5 is almost 2 times as high as that of S1. The possible reasons for the enhancement of emission intensities can be elucidated as follows. On the one hand, the microspheres have an average diameter of 1.2 μm, which is much smaller than the microflowers with an average diameter of 7.5 μm. The building blocks of the two samples vary from 3D dendrites to 0D nanoparticles, the quantum-confinement effect can be used to account for the improvement of emission intensities.28 Moreover, as the particle size is reduced, the ratio of surface Eu3+ is increased, lowering the local symmetry of the crystal field around the Eu3+ ions,29 and thus enhancing the emission intensity. On the other hand, the intrinsic geometry of the microspheres can efficiently minimize the scattering of light from the sample surface as compared with that of other morphologies, further leading to an improvement of emission intensity.30 Therefore, on the basis of the aforementioned explanations, the different luminescence behaviors can be reasonably attributed to the different morphologies and sizes of the two samples.
Accordingly, it is accepted that the obtained La2(MoO4)3 microstructures may also be used as adsorbents to remove organic wastes from water. Herein, as an example, Rhodamine B (Rh B), a widely used dye, was employed as model pollutant to evaluate the adsorption activity of La2(MoO4)3 microstructures. The characteristic absorption of Rh B at 553 nm was selected for monitoring the adsorption process. As shown by the photo images and UV-vis absorption curves at different time intervals in Fig. 10, when the initial concentration of Rh B in water is 10 mg L−1, the La2(MoO4)3 microflowers obtained with the assistance of 0.05 g EDTA could remove about 96.7% of the Rh B without any additives at room temperature. The adsorption capacity of the La2(MoO4)3 microflowers for Rh B was about 48.4 mg g−1. As a comparison, La2(MoO4)3 microspheres (S5) obtained with the aid of 0.46 g EDTA were also selected to detect the removal rate of Rh B. As shown in Fig. 11, the microflowers exhibit a relatively high adsorption rate compared to the microspheres, although the adsorption capacities of two samples are almost the same. Since the BET surface area of microspheres (34.28 m2 g−1) is higher than that of microflowers (22.00 m2 g−1), the enhancement of adsorption rate can be attributed to the novel hierarchical superstructure of microflowers assembled by numerous dendrites. As a result of the self-assembly of a large number of interwoven nanoflakes, the hierarchical microflowers have plenty of meso- and macro-pores (see Fig. SI7 and corresponding description in the Supporting Information†), providing efficient transport paths for adsorption.32 It was reported that chemical reactions can occur more easily when the transport paths through which molecules move into or out of the nanostructured materials are included as an integral part of the architectural design.33 Therefore, in the present work, the presence of efficient transport paths in La2(MoO4)3 microflowers benefits the enhancement of adsorption performance for the removal of Rh B.
Fig. 10 (a) Photo images of absorption of Rh B at different times by La2(MoO4)3 microflowers obtained with the assistance of 0.05 g EDTA. (b) Absorption spectra of a solution of Rh B (10 mg L−1, 50 mL) in the presence of 10 mg La2(MoO4)3 microflowers at different time intervals. |
Fig. 11 Adsorption rate of Rh B on La2(MoO4)3 microflowers with an average size of 7.5 μm (S1) and microspheres with an average size of 1.2 μm (S5). |
As stimulated by the potential applications of the obtained products, the PL properties of the Eu-doped La2(MoO4)3 superstructures with different morphologies were measured. The results revealed that La2(MoO4)3:Eu microspheres constructed by nanoparticles displayed a stronger emission than La2(MoO4)3:Eu microflowers built from interwoven dendrites. Furthermore, to expand the application fields of La2(MoO4)3 hierarchical architectures, the adsorption activity of La2(MoO4)3 as an absorbent in water treatment was also investigated. It was found that the microflowers exhibited a relatively high adsorption rate compared to the microspheres, although the adsorption capacities of two samples are almost the same. Possible reasons responsible for the differences in PL properties and absorption activities of different hierarchical architectures were discussed. It was demonstrated that the PL properties and adsorption activities of the La2(MoO4)3 hierarchical architectures were strongly correlated with the morphology and size, further emphasizing the importance of rational shape control. This work could be of great significance for the exploration and expansion of potential applications of La2(MoO4)3, an outstanding advanced function material.
Footnote |
† Electronic supplementary information (ESI) available: Additional XRD patterns, SEM images and adsorption-desorption isotherms. See DOI: 10.1039/b9nr00392d |