aDepartment of Chemistry, Texas A&M University, College Station, Texas 77842-3012, USA. E-mail: zhou@chem.tamu.edu
bDepartment of Material Science and Engineering, Texas A&M University, College Station, Texas 77843, USA
First published on 2nd September 2015
Kinetic labilization of the Fe(III)–O coordination bond in a mesoporous metal–organic framework, PCN-333-Fe(III), is realized by the reduction of Fe(III) by Cr(II). The Fe(II)–Cr(II) metathesis is thus completely achieved followed by this reductive labilization process that generates PCN-333-Cr(III). The kinetic inertness of Cr(III) provides PCN-333-Cr(III) with enhanced chemical stability as well as a broader range of applications compared to those of PCN-333-Fe(III). For instance, alkylamine incorporated PCN-333-Cr(III) demonstrated significant carbon dioxide uptake while PCN-333-Fe(III) lost its crystallinity after alkylamine treatment.
Based on the Hard and Soft Acid and Base (HSAB) principle,28 chemically robust MOFs can be constructed with carboxylate ligands, hard Lewis bases, and high valence metal ions, such as Fe(III), Cr(III) or Zr(IV), categorized as hard Lewis acids. Compared with MOFs composed of divalent species, many of these high valence metal-containing MOFs can survive in water, or even acid or base solutions. This phenomenon has been extensively demonstrated in the MIL series, UiO series and PCN-22X series.9–15,26 A recent example is an iron based mesoporous MOF, PCN-333-Fe(III), which is stable in both acidic and basic aqueous solutions despite its ultrahigh porosity (Fig. 1).8 However, MOFs constructed with high valence metal ions may suffer from structure breakdown in some specific environments, for instance, PCN-333-Fe(III) totally loses its crystallinity and porosity in alkylamine solution. Incorporation of kinetically inert metal ions, for example, Cr(III), into the framework backbone could generate MOFs with exceptional stability.16,26
Fig. 1 (a) PCN-333 is composed of trimeric clusters and TATB ligands with (b) supertetrahedra as supermolecular building blocks. (c) The small cage with a diameter of 4.2 mm and (d) the large cage with a diameter of 5.5 nm in the construction of (e) the network with MTN topology.8 |
Nevertheless, obtaining crystalline Cr(III)-MOFs with carboxylate ligands are extremely difficult due to the kinetic inertness of Cr(III). Hydrothermal conditions are exclusively adopted in the synthesis of crystalline Cr(III)-MOFs, but these conditions might be unfeasible when using larger organic ligands as they are extremely hydrophobic. Attempts to synthesize PCN-333-Cr(III) using either hydrothermal or solvothermal conditions with temperatures as high as 220 °C failed to generate any crystalline products. An alternative synthetic pathway is the post synthetic metathesis of metal clusters from a template MOF with a known structure. Fe(III)-MOFs can serve as practical structural templates because iron resembles chromium in both coordination geometry and valence. Disappointingly, the metathesis of PCN-333-Fe(III) with CrCl3 for 24 hours only yielded partially metathesized MOF. The incompleteness of the above metathesis is not surprising since in several reports demonstrating the feasibility of metal metathesis for high valance MOFs, complete metal metathesis has never been achieved.24 This is mainly attributed to two reasons: (a) the dissociation of high valence metal ions from a framework is thermodynamically unfavorable; (b) the dissociation rate of high valence ions is much slower than that of divalent species due to the much higher activation energy.25 Therefore, a long reaction time or elevated reaction temperature is required in order to achieve complete metathesis. However, under these scenarios, framework decomposition is usually inevitable due to the acidic environments generated by high valence species.17,25
Herein, we report a reductive labilization–metathesis route for the synthesis of PCN-333-Cr(III) using PCN-333-Fe(III) as the template, wherein redox chemistry contributes to the generation of labile metathesis intermediates. PCN-333-Cr(III) demonstrated a broader range of applications than PCN-333-Fe(III) in consequence of its improved chemical stability. Alkylamine incorporated PCN-333-Cr(III) demonstrated significant CO2 adsorption capacity at low pressure whereas PCN-333-Fe(III) barely shows any CO2 adsorption capacity due to structural decomposition in alkylamine solution.
Fe3+ + Cr2+ → Fe2+ + Cr3+ | (1) |
Driven by the concentration gradient, the metal metathesis between Fe(II) in the intermediate framework and Cr(II) in the solution is favorable.
Freshly prepared PCN-333-Fe(III) was dispersed in a solution of CrCl2 in dry N,N-dimethylformamide (DMF) at 85 °C under the protection of N2. The color of the solid turned gradually from reddish brown to deep green (Fig. 2B). The complete metathesis of Fe by Cr was obtained after 30 minutes as confirmed by inductively coupled plasma mass spectrometry (ICP-MS) and energy-dispersive X-ray spectroscopy (EDS) (Fig. 2A and Table S1†). The SEM-EDS mapping with 4000000 counts results indicated that Cr, C, O and Cl were uniformly distributed on the crystal surface (Fig. 2D–F and S2†). After that, the solids were washed with DMF three times in air to guarantee that all of the Cr(II) ions in the framework were oxidized to Cr(III), which was verified using X-ray photoelectron spectroscopy (XPS) (Fig. S12†). The crystallinity of the metathesized product was maintained and recognized to be isostructural with PCN-333-Fe(III) as shown in the powder X-ray diffraction patterns (Fig. 3, bottom). The surface area and porosity of the metathesized product was also preserved based on the isotherms of N2 adsorption measurements (Fig. 3, top). These reaction conditions are optimized since higher or lower temperatures with longer or shorter reaction times will either yield partially metathesized material or cause structure decomposition and porosity loss.
Fig. 3 N2 isotherms (top) and PXRD patterns (bottom) of PCN-333-Fe(III), PCN-333-Cr(III), PCN-333-Cr(III) treated with water, pH = 0 and pH = 11.0 aqueous solutions for 24 hours. |
The reductive labilization–metathesis process was facilitated in the PCN-333 system due to several structural characteristics. First, the microcrystalline and mesoporous nature of PCN-333 allows the metal ions to diffuse efficiently into the inner cavity of the framework. Besides, the trimeric clusters in PCN-333 are able to accommodate both di- and trivalent metal ions by varying the charges of the terminal ligands, the bridging oxygen atoms, and/or the number of counterions.24 Furthermore, the usage of the anhydrous reaction solvent decelerated the hydrolysis of the Cr(III) species. The absence of acidic conditions contributes to the structural intactness of the intermediate MOF composed of Cr(II)–O bonds.
In order to exclude the possibility that the metathesis of PCN-333-Fe(III) with CrCl2 circumvented the reductive labilization mechanism, a redox inert isostructural framework PCN-333-Sc was synthesized as a template to metathesize with CrCl2. If the Cr(II) species were hypothesized to metathesize with Fe(III) ions in the framework directly without undergoing a redox reaction, complete metal metathesis should also be observed in the system of PCN-333-Sc and Cr(II) since the Sc(III)–O coordination bond is more labile than the Fe(III)–O bond.25 The mixture of PCN-333-Sc and CrCl2 in dry DMF was heated at 85 °C for 30 minutes. The EDS results showed that only one fifth of the scandium in the framework was exchanged with chromium (Table S2†). This observation suggests that the metathesis between PCN-333-Fe(III) and CrCl2 should proceed in a reductive labilization–metathesis manner since a more labile framework failed to generate a completely metathesized product without reductive labilization.
According to Marcus theory and some calculation results, the electron transfer between Fe(III) and Cr(II) in this case should follow an outer-sphere mechanism27 although the experimental evidence of this mechanism is still being pursued in our group. First of all, an inner-sphere mechanism requires the dissociation of axial ligands from Fe(III) whereas an outer-sphere mechanism does not include coordination bond dissociation. Since the dissociation of Fe(III)–ligand bonds is thermodynamically and kinetically unfavorable, an outer-sphere electron transfer mechanism is more reasonable. Moreover, based on calculations, the rate constant of the cross redox reaction between Fe(III) and Cr(II) in aqueous solution is nearly 3 × 107 M−1 S−1, which is close to the rate constant of well-known outer-sphere redox couples, for example, [Fe(phen)3]2/3+ (1.5 × 107 M−1 S−1),27 and much larger than well-known inner-sphere redox couples, for example, [Cr(H2O)6]2+ + [Co(NH3)5Cl]2+ (1.46 × 10−2 M−1 S−1). The metal ions are still in high-spin electronic configurations and their coordination field splittings in the framework or in DMF solutions are similar to those in aqueous solutions, which indicates that outer-sphere electron transfer is expected between these two metal ions.
As expected, the chemical stability of PCN-333-Cr(III) is much more enhanced compared with that of PCN-333-Fe(III). Suspended in water, HCl aqueous solution (pH = 0.0) and NaOH aqueous solution (pH = 11.0) at room temperature for 24 hours, PCN-333-Cr(III) maintained structural integrity without an appreciable loss of crystallinity as confirmed from PXRD measurements (Fig. 3, bottom). In contrast, PCN-333-Fe(III) was only stable in aqueous solutions at pH ranging from 3.0 to 9.0. To demonstrate the intactness of porosity, N2 isotherms were conducted before and after each treatment. The results indicated that the void volume accessibility, the characteristic mesoporous adsorption feature and the pore size distributions of PCN-333-Cr(III) after each treatment were unequivocally preserved (Table S4, Fig. S3–S7†). Remarkably, the samples after each treatment even showed higher total adsorption amounts than the as-prepared PCN-333-Cr(III). That is probably because some insoluble Cr(III) compounds, generated during metal metathesis and trapped in the pores, were removed upon the above mentioned treatments.
The above results have clearly demonstrated that employing kinetically inert metal ions is an efficient strategy for constructing ultrastable MOFs with high porosity. Since the association–dissociation equilibrium of metal–ligand coordination bonds always exists, coordination bonds in a MOF also undergo an association–dissociation process. In aqueous solution, carboxylate ligand substitution around metal ions with other ligands from the solution, for example, water or hydroxyl groups, may take place, which could lead to the breakdown of the MOF structure. For two metal ions with the same valence, the ligand substitution rate of the kinetically inert species is far slower than that of the labile counterpart.25 As shown in Table 1, the ligand exchange rate of Cr(III) in aqueous solution is much slower than that of the Fe(III) species, which is believed to be the key factor that contributes to the superior chemical stability of Cr(III)-MOFs compared with other MOFs based on trivalent species. Meanwhile, the slow Cr–ligand dissociation rate also decreases the hydrolysis rate of the carboxylate ligand which also contributes to the improvement of MOF stability.
Inert complexes | Labile complexes | ||||
---|---|---|---|---|---|
M(OH2) | Cr(OH2)63+ | Ir(OH2)63+ | V(OH2)63+ | Fe(OH2)63+ | Ti(OH2)63+ |
k (s−1) | 2.4 × 10−6 | 1.1 × 10−10 | 8.7 × 101 | 1.6 × 102 | 1.8 × 105 |
By taking advantage of the superior chemical stability of PCN-333-Cr(III), alkylamine was incorporated in PCN-333-Cr(III) with the aim of improving the CO2 adsorption capacity. Branched polyethylenimine (PEI, Mw = 800) was selected due to the high density of amine groups in each molecule. After PEI treatment, the solid maintained its crystallinity with a CO2 adsorption capacity of 8.4 wt% at 1 bar (Fig. S8†). In contrast, PCN-333-Fe(III) completely lost its crystallinity and porosity after PEI treatment according to the PXRD pattern and N2 adsorption measurements (Fig. S9 and S10†).
Powder X-ray diffraction (PXRD) was carried out with a BRUKER D8-Focus Bragg-Brentano X-ray powder diffractometer equipped with a Cu sealed tube (λ = 1.54178 Å) at 40 kV and 40 mA. Thermogravimetric analyses (TGA) were conducted on a TGA-50 (SHIMADZU) thermogravimetric analyzer. Gas sorption measurements were conducted using a Micrometritics ASAP 2420 system at various temperatures. Inductively coupled plasma-mass spectrometry (laser ablation) was carried out using a Perkin-Elmer DRCII ICP-MS with both solution and laser ablation capabilities.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c5sc02587g |