Aijian
Wang
abc,
Jingbao
Song
a,
Ding
Jia
a,
Wang
Yu
a,
Lingliang
Long
a,
Yinglin
Song
d,
Marie P.
Cifuentes
e,
Mark G.
Humphrey
e,
Long
Zhang
c,
Jianda
Shao
c and
Chi
Zhang
*bce
aChina-Australia Joint Research Center for Functional Molecular Materials, Scientific Research Academy, Jiangsu University, Zhenjiang 212013, P. R. China
bChina-Australia Joint Research Center for Functional Molecular Materials, School of Chemical and Material Engineering, Jiangnan University, Wuxi 214122, P. R. China. E-mail: chizhang@jiangnan.edu.cn; Fax: (+86)-510-85917763
cKey Laboratory of Materials for High-Power Laser, Shanghai Institute of Optics and Fine Mechanics, Chinese Academy of Sciences, Shanghai 201800, P. R. China. E-mail: czhang@siom.ac.cn
dSchool of Physical Science and Technology, Soochow University, Suzhou 215006, P. R. China
eResearch School of Chemistry, Australian National University, Canberra, ACT 2601, Australia. E-mail: chi.zhang@anu.edu.au
First published on 8th December 2015
Reduced graphene oxide-tin porphyrin (RGO-SnTPP) nanohybrids with good dispersibility have been prepared by two covalent functionalization approaches. The microscopic structure and morphology of the RGO-SnTPP nanohybrids were characterized by various spectroscopic techniques including Fourier transform infrared spectroscopy, Raman spectroscopy, transmission electron microscopy, thermogravimetric analysis and X-ray photoelectron spectroscopy. Ground-state absorption and steady-state fluorescence studies indicate considerable π–π interactions and effective photo-induced electron and/or energy transfer from the porphyrin moieties to the RGO. Their nonlinear optical properties were investigated using the Z-scan technique at 532 nm with both picosecond and nanosecond laser pulses. The RGO-SnTPP hybrids were found to exhibit large nonlinear optical responses due to a combination of mechanisms, while significant differences in their nonlinear optical responses were observed, highlighting the influence on photophysical properties of the degree of functionalization and the synthetic approach employed.
Thus far, reports of graphene-based materials are largely restricted to graphene oxide (GO), which has chemically reactive oxygen functionalities, including carboxyl, epoxy, and hydroxyl groups; however, it is electrically insulating due to the disrupted sp2 bonding network, and is therefore unfavorable for the construction of optoelectronic devices.8,9 The electrical conductivity and electron transfer properties of graphene can be partially recovered on proceeding from GO to reduced graphene oxide (RGO), the key reduction step restoring the π network. Grafting organic moieties onto the surface of RGO can proceed with retention of the structural integrity of the RGO framework, thereby eliminating the problematic loss of electronic structure.10 Chemical functionalization may therefore potentially pave the way for the use of RGO in practical applications. However, few reports have investigated the covalent chemical modification of RGO compared to the numerous reports of functionalization of GO, perhaps due to the reduced solubility of the former in the absence of electrostatic or steric protection, rendering further processing more difficult.11 It is therefore of significant interest to design and prepare RGO-based solution-processed organic materials for further applications.
Some GO- and porphyrin-based nanohybrids with excellent optoelectronic properties have been reported,4–6 but as yet, there has been no report of axially functionalized porphyrin-RGO nanohybrid materials. Encouraged by these considerations, we report herein two covalent functionalization approaches for the fabrication of RGO-TPP nanohybrid materials. These are based on the initial covalent introduction of phenol groups onto the RGO surfaces by 1,3-dipolar cycloaddition or a diazotization reaction, and subsequent nucleophilic substitution at dichloro(5,10,15,20-tetraphenylporphyrinato)tin(IV) (SnTPP). This covalent grafting of RGO with porphyrin is aimed at optimizing the RGO dispersion and enhancing interfacial bonding. The nanohybrid materials thus prepared are stable in solution and have been characterized by a variety of physical and spectral techniques. We have also explored the potential of combining porphyrin and RGO in a composite material to achieve increased nonlinear optical (NLO) activity. To the best of our knowledge, this is the first report of the fabrication and study of the photophysical and NLO properties of RGO nanohybrids covalently functionalized by axially-coordinated metal-porphyrins.
Fig. 1 Photographic image of the samples dispersed in DMSO (from left to right: RGO, RGO-SnTPP 1, and RGO-SnTPP 2). |
The Raman spectrum of RGO displays the typically strong tangential resonance absorption band (G band) at 1583 cm−1 and the defect band (D band) at 1349 cm−1 (Fig. 3). The former has been used to estimate the level and distribution of modifications, while the latter has been employed to assess the density of defects and has been used to monitor the covalent functionalization which transforms sp2 to sp3 sites.23 The D and G bands of RGO-SnTPP 1 appear at 1346 and 1581 cm−1, respectively, shifted to slightly lower wavenumbers compared to RGO. In contrast, there is a significant shift to lower energy for the D (1349 to 1337 cm−1) and G bands (1583 to 1569 cm−1) of RGO-SnTPP 2 when compared to the analogous bands in the spectrum of RGO. Functionalization of graphene can result in enhancement of the D to G band intensity ratio (ID/IG).24 In the present case, the SnTPP molecules grafted onto the RGO nanosheets contain a large number of sp2 aromatic carbon atoms. Consequently, although some sp2 carbon atoms in RGO were transformed to sp3 carbon atoms, the numbers are still less than those of the sp2 carbon atoms in the grafted porphyrins, leading to an overall decrease of the intensity ratio (ID/IG) from 1.15 for RGO to 1.12 for RGO-SnTPP 1 and 0.96 for RGO-SnTPP 2, and consistent with a conjugated polymer-covalently grafted RGO functional material.23 The Raman spectra of the RGO-SnTPP nanohybrids display similar modifications, but to different degrees. We have not found clear evidence of any Raman peaks characteristic of the functionalizing moieties, which may be due to either the low level of functionalization or random orientation of the SnTPP appendages rendering the direct detection of moieties on RGO exceedingly difficult. Their effect on the properties of RGO is abundantly clear, however. A simple method has been proposed, i.e., La (nm) = (2.4 × 10−10) × λ4laser(ID/IG) (where La represents the crystallite size and λlaser is the laser excitation wavelength), which allows one to indirectly assess the density of graphene defects in terms of the crystallite size.25 Based on the data in Fig. 4, three sizes were obtained (22.1, 21.5 and 18.4 nm), corresponding to pristine RGO, RGO-SnTPP 1 and RGO-SnTPP 2, respectively. The defect density of RGO-SnTPP 2 is larger (corresponding to a reduced crystallite size) than RGO and RGO-SnTPP 1. Indeed, the smaller size of the RGO-SnTPP nanohybrids compared to those of RGO can be directly observed (Fig. 4). The existence of small nanoparticles distributed on the sheets of RGO-SnTPP 1 and RGO-SnTPP 2 (Fig. 4b and c) confirms the presence of SnTPP, and further supports the presence of covalent bonding between SnTPP and RGO.
TGA characterization was also performed, to assess the thermal stability of the materials. TGA plots of RGO, SnTPP, RGO-SnTPP 1 and RGO-SnTPP 2 are shown in Fig. 5. All samples were exhaustively washed and dried beforehand. RGO displays a weight loss of around 5% between 50 and 800 °C due to the removal of the residual oxygen functionalities, consistent with the reported results that RGO exhibits a similarly good thermal stability as that of pristine graphite.26 Both RGO-SnTPP nanohybrids show some weight loss, consistent with the successful functionalization of RGO by axially-coordinated porphyrins. The thermal stability of RGO-SnTPP 2 is higher than that of RGO-SnTPP 1. At 800 °C, the amount of the RGO-SnTPP 2 residue is 54%, whereas the amount of RGO-SnTPP 1 residue is 26%, both of which are significantly larger than SnTPP (8%) due to the presence of RGO. The TGA results display a good agreement with the XPS results (Fig. 6), further indicating that the surfaces of the RGO nanosheets are coated with different amounts of porphyrin as a result of employing the two different synthetic routes.
Fig. 5 TGA profiles of RGO, SnTPP, RGO-SnTPP 1 and RGO-SnTPP 2 measured in nitrogen (heating rate 10 °C min−1). |
Fig. 6 (a) XPS survey scans of RGO, RGO-SnTPP 1 and RGO-SnTPP 2, and (b) XPS spectra of RGO-SnTPP 1 and RGO-SnTPP 2 in the regions of Sn 3d3/2 and Sn 3d5/2. |
XPS was examined to further investigate the chemical bonding at the surface of RGO following modification, the results being shown in Fig. 6. Only two main peaks, corresponding to the carbon and oxygen species, are observed in the spectrum of RGO (Fig. 6a). After functionalization with porphyrins, the spectra of RGO-SnTPP 1 and RGO-SnTPP 2 exhibited four new peaks, corresponding to Cl 2p, N 1s, Sn 3d3/2 and Sn 3d5/2 (Fig. 6a), which confirms the formation of porphyrin grafted RGO.27 Peaks of RGO-SnTPP 1 corresponding to Sn 3d3/2 and Sn 3d5/2 were observed at 495.0 and 486.3 eV. Due to the different chemical environments following functionalization, the binding energies of Sn 3d5/2 and Sn 3d3/2 in RGO-SnTPP 2 are blue-shifted by 0.2 eV and red-shifted by 0.3 eV, respectively (Fig. 6b). The compositions of the RGO-SnTPP nanohybrids were also determined from the XPS results. The weight fractions of Sn in the samples of RGO-SnTPP 1 and RGO-SnTPP 2 were calculated to be 9.77% and 6.39%, respectively, based on which the SnTPP content in the nanohybrids can be determined to be 59.65% and 39.02%, which indicates that the porphyrin content in the two RGO-SnTPP nanohybrids declines on proceeding from RGO-SnTPP 1 to RGO-SnTPP 2 due to the different functionalization procedures.
With the aim of probing the excited-state electronic interactions of porphyrin moieties and RGO, the fluorescence spectra of SnTPP, RGO-SnTPP 1 and RGO-SnTPP 2 were measured. The fluorescence spectrum of SnTPP undergoes modification following covalent functionalization at RGO (Fig. 8), with Stokes shifts of 173 (SnTPP), 177 (RGO-SnTPP 1), and 176 nm (RGO-SnTPP 2). Electron movement through graphene is close to ballistic at room temperature,30,31 so the Stokes shift in the hybrid system, resulting from the energy loss during the process from S0–S1 transition absorption to S1–S0 transition emission, is therefore less than that of SnTPP. Because RGO does not exhibit a fluorescence signal, the fluorescence of both RGO-SnTPP nanohybrids must be from the porphyrin moieties, which unequivocally confirms the presence of the porphyrin units. Furthermore, the fluorescence intensities of RGO-SnTPP 2 and RGO-SnTPP 1 clearly decrease in the order SnTPP > RGO-SnTPP 1 > RGO-SnTPP 2. This indicates that the quenching of the porphyrin moieties emission in RGO-SnTPP 2 is more effective than that in RGO-SnTPP 1. Experimental results and molecular orbital theory have demonstrated that, due to its unique π-electron systems, RGO is a favorable electron acceptor when directly connected to an appropriate electron donor.32 In RGO covalently linked SnTPP nanohybrid materials, the donor–acceptor interactions between RGO and SnTPP may involve two competitive processes: photo-induced electron and energy transfer from SnTPP to RGO,32 and energy absorbing and electron transporting antenna-like behavior at SnTPP, which could result in fluorescence quenching and energy release. The observed red-shift in the emission maximum for RGO-SnTPP 2 and RGO-SnTPP 1 compared to SnTPP may be ascribed to the confinement of organic dye molecules on the surface of RGO and their interactions with the RGO nanosheets, which reflects the modification of the electronic state of SnTPP induced by RGO as demonstrated in the ground-state absorption spectra. The RGO can provide an ideal network to promote charge transfer in porphyrin-based systems and transport electrons to the collecting surface.
In the present work, an open-aperture Z-scan experiment was used to investigate the NLO responses of RGO and the RGO-porphyrin nanohybrids (RGO-SnTPP 1 and RGO-SnTPP 2) in both the picosecond (ps) and nanosecond (ns) regimes. The ps Z-scan was performed at an excitation wavelength of 532 nm with a 21 ps pulse width, while the ns measurements were carried out at 532 nm with a pulse width of 4 ns. In Fig. 9, the open-aperture Z-scan traces of RGO, RGO-SnTPP 1 and RGO-SnTPP 2 using ps laser pulses are displayed. At the excitation wavelength, all samples exhibit clear saturable absorption responses; that is, the total transmission increases as the sample moves to the higher irradiance at the focal plane. A saturable absorption trace arises when the rate of generation of excited states is equal to the rate of their depletion by stimulated emission and excited relaxation.36 The three samples can therefore effectively suppress low intensity light but allow higher intensity light to pass. For RGO nanosheets, the observed saturable absorption can be ascribed to a relatively slow decay process maintaining occupancy of the conduction band, with further photo-excited electrons being prevented from promotion to this band by Pauli blocking: two photo-excited electrons cannot occupy the same state because of the Pauli exclusion principle.37 Thus, at the focal point, the intensity reaches a maximum, resulting in the observed saturable absorption. In these Z-scan traces, the saturable absorption signal increases on proceeding from RGO to RGO-SnTPP 1 and then RGO-SnTPP 2, with the increased absorption a consequence of the covalent linkage between RGO and the porphyrins, and the results indicating that the saturable absorption can be tuned by varying the synthetic routes, which is in good agreement with the experimental results of thin films containing metallophthalocyanine chlorides.38,39 The RGO-SnTPP nanohybrids are superior to RGO as saturable absorbers in the ps regime due to both the increased saturable absorption and the improved solubility and dispersion stability. Interestingly, this is in sharp contrast to the nonlinear absorption performance of a different GO-SnTPP nanohybrid upon excitation at 532 nm with 21 ps pulses;24 under the latter conditions, the GO-SnTPP nanohybrid exhibits an effective reverse saturable absorption behavior at the focal point, although the differing sample concentrations render comparison with the present study necessarily cautious.
Fig. 9 Open-aperture Z-scan traces of RGO, RGO-SnTPP 1 and RGO-SnTPP 2 in DMSO, obtained under 21 ps, 532 nm laser excitation. |
There is currently considerable interest in using carbon nanotube-based nanohybrids as saturable absorbers.40–42 The optical properties of the RGO-based nanohybrids in this work compare favorably with those of solid poly(methylmethacrylate) (PMMA) composites containing porphyrin-covalently-functionalized multi-walled carbon nanotubes (MWCNT-TPP) and of MWCNT-TPP in DMF;43 specifically, the saturable absorption performance of our nanohybrids is superior to the MWCNT-TPP/PMMA composites and the MWCNT-TPP nanohybrid. However, any further comments are not justified, given the differences in experimental conditions such as wavelength, pulse width, repetition rate, etc.
To gain a deeper insight into the nonlinear absorption responses, open-aperture Z-scan measurements were also performed at 532 nm with nanosecond laser pulses. As shown in Fig. 10, the normalized transmittance curve of RGO exhibits two weaker shoulder peaks along with a valley, corresponding to a transformation from saturable absorption to reverse saturable absorption as the sample moves to the focus of a lens.31 At low input fluence, the saturable absorption originating from Pauli blocking dominates the nonlinear absorption due to the state filling of the interband transitions in the sp2-clusters.44 The excited-state absorption arising from numerous localized sp2 configurations in RGO dominates the nonlinear absorption at high input fluence, resulting in the observed nonlinear absorptive valley.45 For other samples, a dip in the transmission appears at the focus (Fig. 10 and S7†), signaling the occurrence of reverse saturable absorption and hence optical limiting behavior.46 The two RGO-SnTPP nanohybrids are superior at optical limiting to SnTPP, RGO and the control sample (blended RGO and SnTPP) (Fig. 10 and S7†). A similar result has been observed for host–guest systems such as cobalt phthalocyanine/DNA-CTMA (hexadecyltrimethylammonium chloride) surfactant complex and cobalt phthalocyanine/liquid crystals, which exhibited increased NLO properties compared with their precursors due to increases in charge-transfer effects.47 The normalized transmittance of RGO-SnTPP 1 at the focal point, where the input fluence is a maximum, dropped to 67% of the incident intensity, identical within experimental error to the decrease to 66% for a previously-reported graphene nanohybrid covalently functionalized by zinc phthalocyanine.48 However, the RGO-SnTPP 2 exhibits a much deeper valley, suggesting that RGO-SnTPP 2 possesses superior optical limiting performance. These nanohybrids therefore offer an easy way to tailor the NLO properties by judicious choice of the synthetic approach. The RGO-SnTPP nanohybrids have smaller nonlinear absorption responses than the porphyrin/Nafion based nanocomposites in ref. 49, but different mechanisms are believed to be responsible for the observed NLO behavior of the RGO-SnTPP systems and the porphyrin/Nafion based nanocomposites, rendering further comments unwarranted.
Fig. 10 Open-aperture Z-scan traces of RGO, RGO-SnTPP 1, and RGO-SnTPP 2 in DMSO, obtained under 4 ns, 532 nm laser excitation. |
The two-photon absorption coefficients β2 for the nanohybrids, RGO, SnTPP, and the RGO/SnTPP blend were calculated by extrapolating the observed performance to neat material, assuming no contribution from the solvent (Table S1;† as the molecular weights of all but SnTPP are unknown, it is not possible to compare the molecular two-photon absorption cross-sections σ2). While being mindful of the errors associated with these measurements, it is clear that the β2 values increase on proceeding from the components RGO and SnTPP to the nanohybrids, and that the β2 values of the nanohybrids under ns conditions differ significantly from that of the RGO/SnTPP blend.
The improved NLO response can have contributions from various mechanisms such as excited-state absorption, nonlinear scattering and photo-induced electron or energy transfer. With organic dyes, NLO performance can be observed using long excitation pulses due to the radiative lifetimes of the lowest triplet states being sufficiently long that there is a corresponding population build-up in the triplet states.50 In the present case, on excitation with nanosecond laser pulses, the intersystem crossing rate and triplet state lifetime of the porphyrin are significant, resulting in a reverse saturable absorption process. The nanohybrid functionalization may result in the small localized sp2 environments increasing significantly in number, but not interconnecting to form new sp2 carbon clusters in the RGO moiety,51,52 as displayed in Scheme 1 and confirmed by the results of Raman, resulting in the improved excited-state absorption.31 Knowledge of the nature of the nonlinear optical response, as well as the impact of the energy/electron transfer on nonlinearity, is very important;53 in the present case, the photo-induced electron or energy transfer process between porphyrin and RGO that was documented in the fluorescence analysis may also contribute to the nonlinear absorption by fluorescence quenching and energy release.54 Nonlinear scattering is often the strongest contributor to nonlinear absorption in nanomaterials. Work by Li et al. suggests that nonlinear scattering is strongly connected to the thermal conductivity of graphene-based materials.55 In the scattering process, the high intensity laser is dispersed, affording a beam with larger spatial dimensions, and thereby resulting in reduced intensity.56 Effective nonlinear scattering can be observed on the nanosecond time scale, while the efficiency of scattering is largely dependent on the scattering cross-section, and hence the size of the scatterers.34
Based on the saturable absorption and reverse saturable absorption performance of the RGO-SnTPP nanohybrids, we anticipate that several novel RGO-based devices could be eventually realized through the use of concepts from the already well-developed RGO optics research. (1) Attachment of the porphyrin moieties onto the surface of the RGO significantly improves the solubility and ease of processing of these RGO-porphyrin covalently functionalized materials. (2) The improved saturable absorption and reverse saturable absorption render RGO-TPP-related materials suitable for potential applications in ultrafast optical switching, as mode-locking elements, or as optical limiters for nanosecond pulses. (3) The work function of RGO is controlled by the chemical functionalization (and indeed the different synthetic routes), so one can expect such functionalization to lead to the control, tuning and tailoring of the NLO properties of RGO. It may also enable the generation of RGO-based optical devices, which may be comparable to, if not better than, the traditional optical materials.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c5qi00209e |