Liqiang Zhang‡
ab,
Yuecun Wang‡c,
Degang Xie‡c,
Yushu Tangab,
Chunyang Wud,
Lishan Cuiab,
Yongfeng Li*a,
Xiaohui Ning*c and
Zhiwei Shanc
aState Key Laboratory of Heavy Oil Processing, China University of Petroleum, Changping, Beijing 102249, China. E-mail: yfli@cup.edu.cn
bDepartment of Materials Science and Engineering, China University of Petroleum, Beijing 102249, China
cThe Center for Advancing Materials Performance from the Nanoscale (CAMP-Nano), Xi An Jiao Tong University, Xian, 710049, China. E-mail: xiaohuining@mail.xjtu.edu.cn
dSchool of Materials Science and Engineering, Zhejiang University, Hangzhou, Zhejiang 310027, China
First published on 12th January 2016
In this work, an in situ transmission electron microscopy (TEM) study of the electrochemically driven sodiation and desodiation of a CuO nanowire (NW) was performed. Upon sodiation, Na ions first reacted with CuO, yielding a mixture of Cu, Cu2O, and Na2O, and then some Cu2O was subsequently reduced into nanocrystal Cu. The final sodiation product was nanocrystalline Cu mixed with Na2O and Cu2O. Upon extraction of Na+, the nanocrystalline Cu first oxidized into Cu2O and finally transformed back to nanocrystalline CuO. The volume of the CuO NW was found to expand markedly during the first sodiation, but the morphology of the NW remained unchanged during the following cycles. The mechanism by which high-performance CuO NW anodes are used for rechargeable Na ion batteries was analyzed by carrying out an in situ TEM technique based on our results, and this study may be beneficial for designing the optimal structure of the CuO anode, improving its cycle performance, and making CuO more feasible for Na ion batteries.
Understanding the detailed microscopic mechanisms of the electrochemical reaction and material degradation is crucial for designing high-performance CuO anodes for NIBs. In this work, an in situ transmission electron microscopy (TEM) technique was applied to investigate the structural and chemical evolution of CuO NWs during Na+ insertion and extraction, and this investigation has provided an essential understanding of the electrochemical reaction mechanism of CuO NWs serving as anodes for NIBs.
The in situ experiments investigating the electrochemically driven sodiation of the CuO NW were conducted in real time by using an all-solid nanobattery assembled inside the transmission electron microscope, and details of the nanobattery setup can be found in our previous publications.26,27 To confirm the negligible magnitude of the effects of the electron beam on the electrochemical reactions, both beam-on and blank experiments were performed. The in situ electrochemical tests and TEM imaging were carried out by using an in situ electrical testing system, Hysitron PI 95 H1H, inside the Hitachi H9500 TEM operated at 300 keV.
The electrochemical Na-storage properties of the CuO NWs were evaluated by galvanostatic cycling using CR2025-type coin cells. The electrode slurry was made by mixing 75 wt% active material (CuO NW/graphite), 15 wt% acetylene black and 10 wt% polyvinylidene fluoride (PVDF) in N-methyl pyrrolidone (NMP) with magnetic stirring for 2 h. The slurry was then coated onto Ni foam and dried at 100 °C in a vacuum overnight to make the working electrodes. The electrodes were then assembled into half cells in an Ar-filled glove box using an Na foil as the counter electrode and a Celgard 2300 polypropylene membrane as the separator. The electrolyte was 1 M NaPF6 dissolved in ethylene carbonate (EC)/dimethyl carbonate (DMC) (1:1 in volume). The cells were charged and discharged at various current densities between 0.005 and 3.0 V vs. Na/Na+ on a Neware battery tester (Shenzhen, China). The specific capacity of CuO/G was calculated based on the total weight of the CuO NW and graphite. Cyclic voltammetry (CV) scanning was carried out on an Arbin BT2000 system between 0.005 and 3.0 V vs. Na/Na+ at various scan rates using three-electrode beaker cells with Na foil as both the counter and reference electrodes. All of the electrochemical measurements were carried out at room temperature.
Fig. 2(a) shows the typical changes in the microstructure of an intrinsic CuO NW during the first sodiation process. When a potential of −3.5 V was applied, the sodiation (discharging) process of the NW occurred. As the reaction front (marked by the red arrows) propagated from (as shown in the figure) the left end to the right end of the CuO NW, the NW immediately elongated and expanded. The single crystalline pristine CuO NW was immediately transformed into a nanocrystal upon insertion of Na+ (Fig. 2(b)). Since the leading edge of the reaction front propagated longitudinally down the NW, the reaction front also proceeded progressively along the radial direction, i.e., from the surface to the center of CuO NW (Fig. S1, Movie S1†). EDPs for the pristine and sodiated CuO NWs confirmed that the single-crystalline CuO NW was first partially converted to Cu2O, and then decomposed into Cu (Fig. 2(c)). After the first discharge reaction, the contrast between a crystalline core and grey shell was clearly observed in the NW. The diameter of the crystalline core of the CuO NW decreased as the sodiation proceeded (Movie S1†). It took about a half an hour to discharge a NW with an initial length of 1.41 μm and diameter of 52 nm. After the first sodiation process, the CuO NW elongated by ∼20%, its diameter increased by ∼78%, and its total volume expanded by about 232%. The CuO NW clearly experienced a large radial expansion upon insertion of Na+. EDX line scans, at the region of the blue dashed line in Fig. 2(b), revealed the distribution of elements at the reaction front (Fig. 2(d)). Although elemental Cu and Na cannot form any alloy during the sodiation process, Na+ can still diffuse into the CuO lattice and form Na2O with the O2− of CuO; and then the Na2O in the CuO NW could further serve as the diffusion channel for Na+ transport. The maintenance of the integrity of the morphology of the CuO NW after the electrochemical reaction contributed to the stability of the battery. Had the CuO been a bulk material, its pulverization could not have been avoided upon the very large expansion of its volume. During the first sodiation, the NW generated a few nanocrystals dispersed in the amorphous matrix (the inset of Fig. 2(b)), and the EDP characterization showed diffraction rings mixed with the amorphous haloes, which could be indexed as Na2O and Cu mixed with Cu2O phases, which can be defined as Cu1−xCuxO1−(x/2). With the prolonged discharging, the diffraction spots related to CuO became weaker, and finally disappeared. The first discharging process has been shown to include three conversion reactions:24
xNa+ + CuO + xe− → x/2Na2O + Cu1−xCuxO1−(x/2) | (1) |
2Cu1−xCuxO1−(x/2) + (2 − 2x)Na+ + (2 − 2x)e− → Cu2O + (1−x)Na2O | (2) |
Cu2O + 2Na+ + 2e− → 2Cu + Na2O | (3) |
The changes in the morphology of the CuO NW during the electrochemical cycling are shown in Fig. 3(a)–(d). The changes of the EDPs of the CuO NW undergoing sodiation/desodiation cycling are shown in Fig. 3(e)–(h). After the first discharging process, the pristine CuO NW became partially sodiated and transformed to a Cu phase mixed with Cu2O and Na2O (Fig. 3(e)), which was transformed back to the crystalline CuO in the following charging process (Fig. 3(f)). Note that the shape of the sodiated CuO NW remained unchanged during the desodiation, and there was a negligible decrease in the volume (Fig. 3(c)). In the following discharging process (Fig. 3(d)), the crystallized CuO transformed back to Cu, and Cu2O again (Fig. 3(g)), which was finally retransformed back to the crystallized CuO (Fig. 3(h)) in the following charging process as well. The CuO NW was found to undergo irreversible volume changes during the cycling processes, and the desodiated CuO NW could not return to its original state. In addition, the sodiated CuO became quite brittle after cycling, and broke suddenly after the second charging (Fig. S1†) due to a tiny vibration. The cycling performance of the CuO NW can be expressed as follows: decomposition of CuO into Cu2O, and then conversion into metallic Cu upon discharging; and reoxidation of Cu2O and Cu into CuO in the subsequent charging process.
Fig. 3 (a–d) Changes in the morphology of the CuO NW during cycling. (e–h) The changes of the EDPs of the CuO NW undergoing sodiation/desodiation cycling. |
In addition, galvanostatic discharge–charge cycling was performed to directly measure the capacity of the CuO NW electrode during sodiation and desodiation at a constant current rate of 200 mA g−1 in a coin cell. The cyclic voltammograms of the CuO NW electrode at a scan rate of 0.2 mV s−1 are shown in Fig. S2,† and they indicate that the CuO NW underwent multiple phase conversions during cycling. In the first discharging process, three reduction peaks at 1.3, 0.8 and 0.1 V were observed in the potential range of 0.01–3 V, which are attributed to the formation of Cu1−xCuxO1−(x/2), the generation of Cu2O and the final conversion into metallic Cu mixed with Na2O, respectively. In the following charging process, two oxidation peaks appeared at 1.3 and 2.1 V that can be indexed to the formation of Cu2O and restoration of CuO phase, respectively. All of the redox peaks reappeared quite consistently from one cycle to the next, except for a slight shift to higher potential, demonstrating good redox reversibility and structural stability.
Fig. 4 shows a schematic diagram of a CuO NW during the sodiation process. With the volume expansion, the reaction front is illustrated to migrate from the left end to the right end of the NW. The formation of Na2O on the surface is due to the surface diffusion and oxidization of Na+. In some carbon anodes without O2−, similar surface oxide phases (Li2O or Na2O) have also been observed under the in situ TEM electrochemical testing condition,28,29 which indicates that the electron beam may affect the formation of the surface oxide layer. Na+ is not able to extract O2− from CuO to form the surface shell as this process requires a very high input of energy. Instead, Na+ can diffuse into the CuO lattice and form Na2O with the O2− of CuO. The new generated Na2O phase in the sodiated CuO NW could serve as the diffusion channel for Na+ transport. As the migration of Na+, Cu2+ first becomes converted to Cu+, and finally to the metallic Cu. The displacement of the reaction front versus the reaction time is plotted in Fig. S3,† and the diameter of the NW was observed to be ∼40 nm. The nearly parabolic character implies the diffusion of Na+ over a long distance, which is significant in determining the battery performance. The different colors correspond to the different lengths of the NW. Based on the above results, the diffusivity rate of Na+ in the reacted amorphous sections was determined to be in the range of 2–9.3 nm s−1. The wide distribution of diffusivity values is reasonable here. In contrast to a crystal, the atomic structure in an amorphous region is not well defined. When subjected to different conditions, the amorphous NWs will form different structural features, such as different lengths, which can lead to different diffusion rates. Owing to the properties of CuO, Na+ can diffuse into the CuO lattice and the generated Na2O phase becomes diffusion channels for the transport of Na+, and this mechanism is quite different from that used by the Sn- or Si-based anode.30,31 The CuO NWs display no obvious changes in morphology during cycling (except the 1st discharging), so they have a potential to achieve long cycling lifetimes and good reversibility. The exterior Na2O shell on the surface of sodiated CuO NW is the solid electrolyte interface (SEI), which could consume the Na+ and lead to an irreversible capacity loss. In the future, investigators are expected to wrap an exterior protective layer (such as a carbon layer) on the surface of the CuO NW; such a wrap would allow the anode to freely expand while retaining good electrical conductivity and would prevent the cracking and pulverization of the CuO anodes. The above results show that significant challenges still need to be overcome before CuO anodes can be widely utilized in practical NIBs.
Fig. 4 A schematic diagram for one part of CuO NW during the (a) start (b) middle and (c) end of the sodiation process. |
Footnotes |
† Electronic supplementary information (ESI) available: The TEM image of CuO NW after cycling; a CV curve for CuO NW based NIB; plots of the reaction front migration distance vs. the time. See DOI: 10.1039/c5ra24086g |
‡ These authors contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2016 |