Open Access Article
This Open Access Article is licensed under a
Creative Commons Attribution 3.0 Unported Licence

Ga2O3–Cu2O: synthesis, characterisation and antibacterial properties

Iman A. Hassana, Sanjayan Sathasivamab, Husn-Ubayda Islama, Sean P. Nairc and Claire J. Carmalt*a
aMaterials Chemistry Centre, Department of Chemistry, University College London, 20 Gordon Street, London WC1H 0AJ, UK. E-mail: c.j.carmalt@ucl.ac.uk; Fax: +44 (0)20 7679 7463
bBio Nano Consulting Ltd, The Gridiron Building, One Pancras Square, London N1C 4AG, UK. E-mail: info@bio-nano-consulting.com; Fax: +44 (0)20 7396 1056
cDivision of Microbial Diseases, UCL Eastman Dental Institute, 256 Gray's Inn Road, London, WC1X 8LD, UK

Received 4th October 2016 , Accepted 10th December 2016

First published on 3rd January 2017


Abstract

This paper reports on a Ga2O3–Cu2O composite thin film that allows the destruction of both Gram negative and Gram positive bacteria via a dual mechanism involving Ga3+ ions that disrupt Fe3+ metabolism pathways in bacteria as well as through the reactive oxygen species generated by possible Fenton type reactions that are mediated by Cu1+ ions. This dual mechanism allowed the highly transparent composite thin film to destroy both E. coli and S. aureus to below detection limits in 24 hours and limits the build up of bacterial resistance. The composite film was amorphous and the nature of the Ga and Cu species was extensively analysed on the surface and the bulk using X-ray photoelectron spectroscopy and synchrotron radiation involving linear combination analysis (LCA) and the X-ray absorption near edge structure.


Introduction

Hospital acquired infections (HAI) are a major and increasing problem for hospitals and healthcare institutions globally.1 The Centers for Disease Control and Prevention (CDC) estimated that 1 in 20 hospitalised patients contracted HAI resulting in approximately 2 million infections contributing to 100[thin space (1/6-em)]000 deaths a year and costing US hospitals over $30 billion.

The use of conventional antimicrobials to fight such infections is becoming less effective due to the increasing occurrence of multidrug resistant bacteria.2,3 Hospital and health care environments represent a reservoir for multidrug resistant bacteria and therefore new methods for reducing or eliminating microorganisms from these environs using antibacterial coatings consisting of (for example) metals and metal oxides with antibacterial properties on high contact touch surfaces, such as keyboards and door handles, is desirable.4–6

One of the most well known antibacterial agents is Cu in the metallic or oxide form. It has been used for centuries to decontaminate water. The mode of action is complex, but is believed to be through Fenton type reactions that involve the production of reactive oxygen species (ROS) which go on to cause damage to bacterial cell membranes, DNA and proteins through oxidative stress.7,8 Although a potent antibacterial agent, Cu and its oxides are expensive relative to other metals (and metal oxides), thus making the use of Cu costly when application of the coatings on large areas, such as those found in hospitals, is required. Furthermore, the use of Cu or Cu2O, CuO causes aesthetic concerns, as the coatings are not transparent but coloured.

Gallium oxide however is highly transparent in the visible and displays antibacterial activity. Ga has demonstrated harmful effects on microorganisms, particularly in mechanisms involving the metabolism of iron.1 Gallium has been used in biological studies despite having no known physiological functions in the human body. The mechanism for the antimicrobial activity of gallium (Ga3+) has been related to its ability to mimic iron (Fe3+) but not to participate in redox reactions. Gallium is able to compete with iron and interferes with the absorption and activity of Fe3+. Gallium with a trivalent charge (Ga3+) has an ionic radius of ∼0.55 Å that corresponds well with Fe3+ (∼0.5 Å). This can allow Ga3+ to displace Fe3+ in biochemical molecules and pathways. However, iron is redox active but gallium is not. Therefore, the substitution of Fe3+ with Ga3+ will lead to the inactivation of Fe-dependent biomolecules. Iron is important for cell division and essential for the formation of DNA. Therefore disruptions in the absorption of iron can cause the cells not to be able to produce sufficient DNA for replication, which ultimately leads to its death.1–3

Antimicrobial activity of gallium has been demonstrated with in vitro investigation of gallium in the form of gallium maltolate9,10 and gallium nitrate.11,12 Studies have shown that gallium nitrate can inhibit the growth of biofilms. Biofilms were grown in the presence and absence of low concentration of gallium nitrate and it was observed that limiting the presence of Fe in the nutrients had a positive correlation with the concentration of Ga and microbial reduction was observed. However, when Fe was introduced into the medium, competition between the Ga3+ and Fe3+ occurred causing the antimicrobial activity of Ga to decrease.13,14

The antimicrobial activity of Ga3+ was also investigated using Ga2O3-doped phosphate-based glasses (PBGs). PBGs are durable materials used as wound dressings where antibacterial ions are incorporated. This unique system would be able to deliver Ga3+ as the glass degrades. The tests demonstrated that the PBGs had antibacterial effects on different HAI bacterial agents. Results indicated that 1% mol Ga2O3-doped PBG was sufficient to be potent against a range of organisms tested. Investigation on Ga2O3 nanoparticles have shown that they interfere with the adhesion mechanism of bacterial strains and reduce the formation of biofilms.14

The use of a composite Ga2O3–Cu2O film that contains both Ga and Cu ions would allow a dual mode of attack against bacteria via (1) the disruption of bacterial Fe3+ metabolism by Ga3+ ions as well as (2) attack through Cu and ROS. Thus making the development of bacterial resistance unlikely. In addition to this, the composite films rich in Ga remain highly transparent in the visible, unlike pure Cu2O or CuO films, therefore allowing application as coatings in hospital and health care environments. In this paper we show the synthesis, to the best of our knowledge, of the first (film or powder) composite Ga2O3–Cu2O sample and subsequent tests against both Gram-negative and Gram-positive bacteria. The films were prepared using a novel route called aerosol assisted chemical vapour depositon (AACVD) that is simple and easily scalable.15–20 Furthermore, since the as-deposited films were X-ray amorphous characterization was carried out using both X-ray photoelectron spectroscopy and linear combination analysis/X-ray absorption near edge structure to determine the nature of Ga and Cu species on the surface and bulk respectively.

Experimental

Materials and general methods

The precursor solution for all AACVD depositions was placed in a glass bubbler and vaporised by use of a Vicks ultrasonic humidifier. This produced an aerosol of the precursor in the solvent used. Nitrogen (99.99%) carrier gas was used as supplied from BOC. Depositions were carried out on SiO2 coated float-glass that was cleaned using propan-2-ol, acetone and dried in air prior to use. The glass substrates were ca. 90 mm × 45 mm × 4 mm in size. The heating of the glass substrate to the desired temperature was carried out under nitrogen gas and two-way taps were used to divert the nitrogen carrier gas through the bubbler. The aerosol was carried into the reactor in a stream of nitrogen gas through a brass baffle and a top plate was suspended 0.5 cm above the glass substrate to ensure a laminar flow. After all the precursor solution had passed through the chamber the taps were turned to allow only N2 gas flow through the bypass tap. This was maintained until the reaction chamber temperature fell below 100 °C. The N2 gas was stopped and the glass substrates were removed. The N2 gas flow rate was controlled by a calibrated flow meter positioned before the gas enters the bypass bubbler. The total deposition time was in the region of 50–80 min.

A graphite block containing a Whatman cartridge heater was used to heat the glass substrate. The temperature of the substrate was monitored by a Pt–Rh thermocouple. Coated substrates were handled and stored in air. Large pieces of glass (ca. 4 cm × 2 cm) were used for X-ray powder diffraction but the coated substrate was cut into ca. 1 cm × 1 cm squares for subsequent analysis.

GaMe3 were used as supplied from SAFC HiTech. GaMe3 is pyrophoric and hence manipulations were performed under a dry, oxygen-free dinitrogen atmosphere using standard Schlenk techniques or in an Mbraun Unilab glovebox. All solvents and alcohols commercially procured from Aldrich were dried with anhydrous engineering equipment and stored in Young's tap flasks.

Preparation of Ga2O3 film

Dried methanol (30 ml) was added to trimethylgallium [GaMe3, 4.35 mmol] at −78 °C. The resulting solution was mixed under N2 for 30 minutes in the AACVD bubbler. The Ga2O3 films deposited at 450 °C were amorphous.

Preparation of Ga2O3–Cu2O film

Copper nitrate trihydrate ([Cu(NO3)2·3H2O], 2.06 mmol) was added to dried methanol (30 ml) at room temperature and allowed to dissolve. The copper nitrate solution was then slowly added to GaMe3 (4.35 mmol) at −78 °C. After 30 minutes of mixing the solution was used for an AACVD experiment. An aerosol was generated at room temperature. A graphite heating block under the glass substrate heated the CVD reactor to 450 °C. Once deposition was complete, the substrate was cooled to room temperature under N2. The film deposition time was one hour and transparent films covering the glass substrate were produced.

Both films were also deposited on quartz substrates and annealed at 1000 °C for 12 hours under air to subsequently determine the crystallographic phase through X-ray diffraction.

Characterisation of thin films

The resulting thin films were handled and stored in air. The coated glass substrates were used for powder X-ray diffraction (XRD) measured on a Bruker D8 X-ray diffractometer with CuKα1 and CuKα1 radiation of wavelength 0.154056 and 0.154439 nm respectively emitted with an intensity ratio of 2[thin space (1/6-em)]:[thin space (1/6-em)]1, a voltage of 40 kV and current of 40 mA. The samples were indexed using the GSAS programme, refined via the Rietveld method (LeBail model), and compared to database standards. Energy dispersive X-ray analysis (EDX) was obtained on Philips XL30ESEM instrument and Scanning electron microscopy (SEM) on a JEOL 6301 instrument. X-ray photoelectron spectroscopy (XPS) was performed using a Thermo Scientific K-alpha photoelectron spectrometer using monochromatic Al radiation. Samples were earthed using copper tape. Higher resolution scans were recorded for the principal peaks of Cu(2p), Ga(3d, 2p), O(1s) and C(1s) at a pass energy of 50 eV. The peaks were modelled using CasaXPS software with binding energies adjusted to adventitious carbon (284.5 eV) for charge correction.

X-ray absorption spectroscopy (XAS) measurements on the Dutch-Belgian Extended X-ray absorption fine structure (EXAFS) beamline (BM26A) at the ESRF in Grenoble. Monochromatic radiation was supplied by a double Si(111) crystal, and fluorescence was measured using a 9 element germanium solid state detector. XAS of the film was acquired in fluorescence. Measurements of the thin film and pelletized copper standards were taken on the copper K-edge (8987 eV). XAS data were processed and X-ray absorption near edge structure (XANES) analysis was performed using Horae Athena software, and detailed EXAFS analysis was performed on Excurve version 9.273.

Antimicrobial testing

E. coli strain (ATCC 25922) and S. aureus (8325-4) was maintained by weekly subculture on Brain Heart Infusion (BHI) agar (Oxoid, Basingstoke, UK). One bacterial colony of either E. coli or S. aureus was used to inoculate 10 ml of sterile BHI broth (Oxoid, Basingstoke, UK) and incubated aerobically at 37 °C for 24 hours. Bacteria from the overnight culture were harvested by centrifugation at 13[thin space (1/6-em)]000 × g for 1 minute. Bacteria were then re-suspended in phosphate-buffered saline (PBS) (Oxoid, Basingstoke, UK) and again centrifuged for 13[thin space (1/6-em)]000 × g for 1 minute. Finally the bacterial pellet was re-suspended in PBS before use. The turbidity of the bacterial cell suspension was measured at 600 nm using a spectrophotometer and was adjusted to an optical density which corresponded to approximately 105 colony forming units (cfu) per 25 μL aliquot.

Prior to use, the gallium oxide and copper gallium oxide samples were cut into 1 × 1 cm sections. A humidity chamber was created to ensure that the suspensions did not dry out. For each exposure time, triplicate samples were analysed and uncoated barrier glass pieces were used as a control. Each exposure time was also repeated twice. A 25 μl aliquot of the bacterial cell suspension was spread evenly on the surface of each slide and incubated at room temperature (21 ± 2 °C) for the allocated exposure time. After incubation the slides were aseptically transferred to 225 μL PBS and vortexed for 30 seconds to release the bacteria into the solution. Serial dilutions of the resulting bacterial suspensions were prepared in PBS and 25 μL from each dilution was spread on to MacConkey Agar (Oxoid, Basingstoke, UK) for E. coli and BHI agar (Oxoid, Basingstoke, UK) for S. aureus. Plates were allowed to dry before inverting and incubating aerobically at 37 °C for 24 hours. After incubation, any bacterial colonies were counted and the viable count calculated. The Mann–Whitney U test was used to determine the significance of the antimicrobial activity of gallium oxide and copper gallium oxide compared to the control glass slide. As well as, determining the significance of the activity of gallium oxide compared to the copper–gallium oxide.

Results and discussion

Pure Ga2O3 and composite Ga2O3–Cu2O thin films were deposited on glass substrates via aerosol assisted chemical vapour deposition of GaMe3 (4.35 mmol) and [Cu(NO3)2·3H2O] (2.06 mmol) in dry methanol. Deposition temperature of 450 °C was chosen as it allowed both precursors to decompose efficiently, promoting surface reactions while minimizing gas phase decomposition resulting in complete coverage of the substrate. The films were highly transparent in the visible. Both films passed the Scotch™ tape test and were resistant to marking and delamination when scratched with stainless steel and brass styluses. The films also remained unchanged after suspension in water and organic solvents (methanol and acetone) for 16 hours. In fact they were only damaged by concentrated (nitric) acid (less than two hours). The highly robust nature of the films is an important property that makes them suitable as functional coatings on high contact touch surfaces.

The deposited films were amorphous when probed using X-ray diffraction spectroscopy. This is expected as Ga2O3 and related systems only exhibit crystallinity at temperatures of 700 °C and above. Annealing of the as-deposited thin films at 1000 °C (to maximize crystallinity) in air for 12 hours did indeed produce crystalline β-Ga2O3.

The composite film, when annealed, showed the growth of the β-Ga2O3 and CuO phases (Fig. 1). There was no evidence for the formation of the spinel phase that has previously been isolated for AACVD synthesized Ga2O3 and CuO composite films when annealed under vacuum.21 As a result, further discussion in this manuscript will focus solely on the amorphous as-deposited films of pure Ga2O3 and composite Ga2O3–Cu2O.


image file: c6ra24737g-f1.tif
Fig. 1 PXRD patterns of the annealed pure and composite film. The standard patterns for β-Ga2O3 and CuO are also shown.

Energy dispersive X-ray spectroscopy (EDX) showed the composite film to be rich in Ga with only 21 at% being composed of Cu compared to 79 at% Ga. The composite film being Cu poor allows it to remain highly transparent without any colour thus enabling it to be applied as a coating on a wider range of surfaces without any issues with aesthetics.

The nature of the Ga and Cu species on the surface of the amorphous composite film was determined by X-ray photoelectron spectra (XPS). The Ga 2p3/2 and 3d5/2 transitions appear at 1117.9 and 19.9 eV, matching well with literature reports for Ga3+.22,23 The Cu 2p spectrum shows two symmetrical peaks separated by 19.6 eV with a low signal to noise ratio. The Cu 2p3/2 peak centered at 932.6 eV can correspond to Cu0 and/or Cu1+ as both peaks overlap heavily.24,25 The ratio of Ga to Cu on the surface was 7 (86 at%) to 1 (14 at%). This is slightly different to what was observed from EDX, which suggests that there was more Cu present in the bulk of the films compared to the surface. The valence band XPS spectra for both films is shown in Fig. 2d. The valence band of pure Ga2O3 is broad, with a width of ca. 10 eV and generalized gradient approximation GGA of density functional theory (DFT) suggests that it is primarily composed of O 2p states.26 Other calculations (tight binding) have however suggested that the valence band of Ga2O3 may also consist of O 2p, Ga 4p and Ga 4s states.26,27 The composite film shows a similar spectrum to the pure film but is shifted to lower binding energies by ca. 1 eV.


image file: c6ra24737g-f2.tif
Fig. 2 XPS core level spectra for the composite film showing the (a) Ga 2p, (b) Ga 2d and (c) Cu 2p transitions. (d) Shows the valence band spectra.

The oxidation of the Cu and Ga species in the bulk of the pure Ga2O3 and composite Ga2O3–Cu2O films were analysed using linear combination analysis (LCA) and X-ray absorption near edge structure (XANES). Cu K-edge XANES data for the sample is shown in Fig. 3 along with the corresponding data for standard powders: Cu, Cu2O and CuO. The energy scales of all the spectra have been consistently normalised. Fig. 3 shows that the local environment of Cu can have an effect on the line shape of the XANES spectra, therefore making it fairly simple to identify the nature of Cu present in the Ga2O3–Cu2O films. The prominent feature seen in the Cu K-edge spectra (Fig. 3a) is from the allowed 1s to 4p transition.28 A low energy peak situated at ca. 8982 eV matches for Cu(0) species in the Cu standard powder, this peak is shifted to a higher energy of ca. 8985 eV and ca. 8987 eV for Cu(I) (Cu2O standard powder) and Cu(II) (CuO standard powder) respectively. All these peak positions match closely with literature reports.28,29


image file: c6ra24737g-f3.tif
Fig. 3 (a) Normalised Cu K-edge XANES spectra for Cu metal foil, Cu2O, CuO and the Ga2O3–Cu2O composite thin film. (b) K3-weighted χ(k) spectra Ga2O3–Cu2O and theoretical fit. (c) Fourier transform of EXAFS of the χ(k).

In this case, the XANES spectra for the amorphous Ga2O3–Cu2O films match that of Cu, Cu2O and CuO standards indicating that copper is present in the film in all three oxidation states. This is in contrast to the surface of the film that XPS analysis showed to be lacking in CuO. LCA for the Ga2O3–Cu2O (Table 1) calculated the Cu[thin space (1/6-em)]:[thin space (1/6-em)]Cu2O[thin space (1/6-em)]:[thin space (1/6-em)]CuO ratio present in the film is 0.37[thin space (1/6-em)]:[thin space (1/6-em)]0.60[thin space (1/6-em)]:[thin space (1/6-em)]0.03. The XANES data indicates that Cu, Cu2O and a very small amount CuO were identified. XPS only identified the presence of Cu2O on the surface of the material. This could be due to CuO not being present at the surface but can be detected in the bulk of the film. The LCA also shows that Cu2O has the largest amount in the ratio, which corresponds to the identification that the composite is a Ga2O3–Cu2O material.

Table 1 Linear combination analysis (LCA) of XANES fit for the amorphous Ga2O3–Cu2O composite film grown via AACVD at 450 °C
LCA of XANES of Ga2O3–Cu2O
Standard Ratio R-factor
Cu2O 0.60 (0.03) 2.51 × 10−4
CuO 0.03 (0.02)
Cu 0.37 (0.02)

EXAFS fit of Ga2O3–Cu2O
Scatter N RXRD (Å) REXAFS (Å) σ22) F
O 2.0 1.85 (Cu2O) 1.87 (0.03) 0.010 12
1.95 (CuO)
Cu 4.6 2.54 (Cu) 2.55 (0.02) 0.010


EXAFS were analysed and revealed the presence of two distances (Table 1). The local structure of Cu2O with two Cu–O distances that were found to be 1.87 Å, which corresponds to bond distances found in Cu2O (1.85 Å). The Cu–Cu distances were identified as 2.55 Å, which is comparable to Cu–Cu bond distance found in pure copper films (2.54 Å).

An important factor that determines efficiency of antibacterial coatings is the surface area. A more nano- and micro-structured morphology of an active film allows it to rapidly destroy bacteria purely through increased contact. This is the primary reason why nano powders show increased activity compared to bulk powders of the same materials. Scanning electron microscopy (SEM) was used to determine the surface topography of both the as-deposited Ga2O3 and Ga2O3–Cu2O amorphous films and give only a qualitative indication of the differing surface area. The Ga2O3 film consists of fused particles roughly 100 nm in diameter. This film appeared to have a larger surface area compared to the composite film that showed much larger particle sizes at 400 nm (Fig. 4). Cross sectional SEM imaging showed both films to be 500 nm thick.


image file: c6ra24737g-f4.tif
Fig. 4 SEM images of the (a) pure Ga2O3 film and (b) composite Ga2O3–Cu2O grown via AACVD on glass substrates from the reaction of GaMe3 and Cu(NO3)2·3H2O in methanol. The cross-sectional SEM image of each film is also shown as an inset.

Optical properties of the Ga2O3 and composite Ga2O3–Cu2O were studied by transmission and reflectance measurements between 300–2500 nm by UV-Vis spectroscopy (Fig. 5). Both of the amorphous films showed a slight shift in the adsorption edge towards the visible relative to plain glass substrate and displayed minimal reflectively (10–20%). The Ga2O3 films displayed high transmission (85–90%) whereas the composite was slightly lower in transmission (80–85%).


image file: c6ra24737g-f5.tif
Fig. 5 UV-Vis spectra for the pure Ga2O3 and the composite Ga2O3–Cu2O thin films grown on glass from the AACVD reaction of GaMe3 and Cu(NO3)2·3H2O in methanol at 450 °C. Inset is a photograph of the films showing the high transparency in the visible.

The antimicrobial properties of the amorphous Ga2O3 and Ga2O3–Cu2O films deposited from GaMe3 in methanol or a mixture of GaMe3 and [Cu(NO3)2·3H2O] via AACVD at 450 °C were tested against E. coli and S. aureus. Samples were cut in 1 × 1 cm sample sections and were covered with 25 μL of bacterial cell suspension containing approximately 105 cfu. Through enumeration and plating of the bacterial suspensions and subsequent overnight incubation (37 °C), the resultant viable counts of bacteria for each sample section was determined. The results for the Ga2O3 and Ga2O3–Cu2O films, shown in Fig. 5, demonstrate that the films have antimicrobial activity against E. coli and S. aureus. Glass cut into 1 × 1 cm were used as controls. Each point represents the log10 of the mean number of viable bacteria from three samples and error bars represent the standard error. The results for the films show that having both Ga and Cu in the films has an enhancing effect on the antimicrobial activity.

For E. coli, a 0.9[thin space (1/6-em)]log10 reduction (P < 0.01) in viable bacteria was observed after 24 hours, for Ga2O3, as shown in Fig. 6a. In the case of Ga2O3–Cu2O, the same reduction in colony counts was achieved after only 9 hours (P < 0.001) and 4[thin space (1/6-em)]log10 reduction was observed after 24 hours. This was similar for S. aureus, a 1.2[thin space (1/6-em)]log10 reduction (P < 0.001) for Ga2O3 was observed after 24 hours however, for the Ga2O3–Cu2O samples a 0.8[thin space (1/6-em)]log10 reduction was observed after 9 hours (P < 0.001) and 4[thin space (1/6-em)]log10 reduction after 24 hours (P < 0.001). When the antimicrobial activity of the Ga2O3 thin films prepared in this study are compared to previous studies where Ga2O3-doped phosphate-based glasses were tested against Pseudomonas aeruginosa a similar reduction in the viable count was seen (0.86[thin space (1/6-em)]log10 reduction).9,10 Overall Ga2O3 has been demonstrated to have some antimicrobial activity. With the Ga2O3–Cu2O film, a much greater bacterial reduction was observed. When comparing the difference in the viable count between Ga2O3 and Ga2O3–Cu2O, it was seen to be highly statistically significant (P < 0.001) demonstrating the impact of copper on the sample. The Ga2O3–Cu2O has a much improved antimicrobial efficacy over Ga2O3 due to the addition of an antimicrobial metal, copper in a mixture of Cu2O. Copper has been shown to produce highly significant reductions in the number of bacteria responsible for HAI. The results herein show that Ga2O3–Cu2O coatings have lower antimicrobial activity compared to Cu and Cu2O coatings.5 It has been shown that copper coatings can reduce bacterial numbers in 30 minutes rather than 24 hours. However, the Ga2O3–Cu2O films we developed were transparent and have the potential to be deposited on a wide variety of surfaces.


image file: c6ra24737g-f6.tif
Fig. 6 The antibacterial properties of the pure Ga2O3 and composite Ga2O3–Cu2O thin films as tested against (a) E. coli and (b) S. aureus.

Conclusions

In conclusion we report the first synthesis and material characterization of a Ga2O3–Cu2O composite. The amorphous thin films were characterized using XPS to indicate that the surface was composed of Ga and Cu in the 3+ and 1+ oxidation state at a ratio of 7[thin space (1/6-em)]:[thin space (1/6-em)]1. The bulk of the film was determined via LCA and XANES analysis to consist of Ga3+ and primarily Cu1+. A small amount of Cu0 and Cu2+ was also found. The presence of both Ga3+ and Cu1+ in the composite film allowed it to display superior antibacterial activity against both Gram negative (E. coli) and Gram positive (S. aureus) bacteria with kills to below the detection limits obtained within 24 hours. Whereas the pure Ga2O3 film tested under the same conditions showed only a ∼1[thin space (1/6-em)]log10 reduction over this time period. The enhanced activity of the composite film was attributed to the dual mechanism of attack involving both the Ga3+ ions (disrupting the vital Fe3+ metabolic pathway of bacteria) and Cu1+ (via Fenton type reactions that produce ROS). The dual mechanism of attack also makes it unlikely that bacterial resistance will arise, an important quality in recent times where the occurrence of multidrug resistant bacterial is major concern. Furthermore, the synthesis of the highly transparent films carried out using the facile AACVD route allows the composite films to be easily applied to large surfaces at limited cost and difficulty.

Acknowledgements

The EPSRC are thanked for studentship funding (IAH) through the Molecular Modelling and Materials Science Doctoral Training Centre (grant EP/G036675).

References

  1. V. Musat, B. Teixeira, E. Fortunato, R. C. C. Monteiro and P. Vilarinho, Surf. Coat. Technol., 2004, 180, 659–662 CrossRef.
  2. M. W. Climo, D. S. Yokoe, D. K. Warren, T. M. Perl, M. Bolon, L. A. Herwaldt, R. A. Weinstein, K. A. Sepkowitz, J. A. Jernigan and K. Sanogo, N. Engl. J. Med., 2013, 368, 533–542 CrossRef CAS PubMed.
  3. K. Page, R. G. Palgrave, I. P. Parkin, M. Wilson, S. L. P. Savin and A. V. Chadwick, J. Mater. Chem., 2007, 17, 95–104 RSC.
  4. S. Noimark, J. Weiner, N. Noor, E. Allan, C. K. Williams, M. S. P. Shaffer and I. P. Parkin, Adv. Funct. Mater., 2015, 25, 1367–1373 CrossRef CAS.
  5. I. A. Hassan, I. P. Parkin, S. P. Nair and C. J. Carmalt, J. Mater. Chem. B, 2014, 2, 2855–2860 RSC.
  6. A. M. Alotaibi, S. Sathasivam, S. P. Nair and I. P. Parkin, J. Mater. Chem. B, 2016, 4, 666–671 RSC.
  7. J. P. Ruparelia, A. K. Chatterjee, S. P. Duttagupta and S. Mukherji, Acta Biomater., 2008, 4, 707–716 CrossRef CAS PubMed.
  8. C. E. Santo, P. V. Morais and G. Grass, Appl. Environ. Microbiol., 2010, 76, 1341–1348 CrossRef CAS PubMed.
  9. C. E. Arnold, A. Bordin, S. D. Lawhon, M. C. Libal, L. R. Bernstein and N. D. Cohen, Vet. Microbiol., 2012, 155, 389–394 CrossRef CAS PubMed.
  10. M. Coleman, K. Kuskie, M. Liu, K. Chaffin, M. Libal, S. Giguère, L. Bernstein and N. Cohen, Vet. Microbiol., 2010, 146, 175–178 CrossRef CAS PubMed.
  11. C. R. Chitambar, Future Med. Chem., 2012, 4, 1257–1272 CrossRef CAS PubMed.
  12. C. R. Chitambar, D. P. Purpi, J. Woodliff, M. Yang and J. P. Wereley, J. Pharmacol. Exp. Ther., 2007, 322, 1228–1236 CrossRef CAS PubMed.
  13. M. Frezza, C. N. Verani, D. Chen and Q. P. Dou, Lett. Drug Des. Discovery, 2007, 4, 311–317 CrossRef CAS.
  14. S. P. Valappil, D. Ready, E. A. A. Neel, D. M. Pickup, L. A. O'Dell, W. Chrzanowski, J. Pratten, R. J. Newport, M. E. Smith and M. Wilson, Acta Biomater., 2009, 5, 1198–1210 CrossRef CAS PubMed.
  15. N. Chadwick, S. Sathasivam, A. Kafizas, S. M. Bawaked, A. Y. Obaid, S. Al-Thabaiti, S. N. Basahel, I. P. Parkin and C. J. Carmalt, J. Mater. Chem. A, 2014, 2, 5108–5116 CAS.
  16. S. Ponja, S. Sathasivam, N. Chadwick, A. Kafizas, S. M. Bawaked, A. Y. Obaid, S. Al-Thabaiti, S. N. Basahel, I. P. Parkin and C. J. Carmalt, J. Mater. Chem. A, 2013, 1, 6271–6278 CAS.
  17. S. D. Ponja, S. Sathasivam, I. P. Parkin and C. J. Carmalt, RSC Adv., 2014, 4, 49723–49728 RSC.
  18. S. Sathasivam, R. R. Arnepalli, K. K. Singh, R. J. Visser, C. S. Blackman and C. J. Carmalt, RSC Adv., 2015, 5, 11812–11817 RSC.
  19. S. Sathasivam, R. R. Arnepalli, D. S. Bhachu, Y. Lu, J. Buckeridge, D. O. Scanlon, B. Kumar, K. K. Singh, R. J. Visser and C. S. Blackman, J. Phys. Chem. C, 2016, 120, 7013–7019 CAS.
  20. D. S. Bhachu, S. J. A. Moniz, S. Sathasivam, D. O. Scanlon, A. Walsh, S. M. Bawaked, M. Mokhtar, A. Y. Obaid, I. P. Parkin and J. Tang, Chem. Sci., 2016, 7, 4832–4841 RSC.
  21. C. E. Knapp, I. D. Prassides, S. Sathasivam, I. P. Parkin and C. J. Carmalt, ChemPlusChem, 2014, 79, 122–127 CrossRef CAS.
  22. B. Cheng and E. T. Samulski, J. Mater. Chem., 2001, 11, 2901–2902 RSC.
  23. S. Sathasivam, R. R. Arnepalli, B. Kumar, K. K. Singh, R. J. Visser, C. S. Blackman and C. J. Carmalt, Chem. Mater., 2014, 26, 4419–4424 CrossRef CAS.
  24. M. C. Biesinger, L. W. M. Lau, A. R. Gerson and R. S. C. Smart, Appl. Surf. Sci., 2010, 257, 887–898 CrossRef CAS.
  25. A. M. Alotaibi, S. Sathasivam, S. P. Nair and I. P. Parkin, J. Mater. Chem. B, 2016, 4, 666–671 RSC.
  26. H. He, M. A. Blanco and R. Pandeyb, Appl. Phys. Lett., 2006, 88, 261904 CrossRef.
  27. E. A. Albanesi, S. J. Sferco, I. Lefebvre, G. Allan and G. Hollinger, Phys. Rev. B: Condens. Matter Mater. Phys., 1992, 46, 13260 CrossRef CAS.
  28. A. Gaur, B. D. Shrivastava and S. K. Joshi, J. Phys.: Conf. Ser., 2009, 190, 012084 CrossRef.
  29. L. S. Kau, D. J. Spira-Solomon, J. E. Penner-Hahn, K. O. Hodgson and E. I. Solomon, J. Am. Chem. Soc., 1987, 109, 6433–6442 CrossRef CAS.

This journal is © The Royal Society of Chemistry 2017
Click here to see how this site uses Cookies. View our privacy policy here.