A polycaprolactone/fish collagen/alginate biocomposite supplemented with phlorotannin for hard tissue regeneration

JeongHyeong Ima, Chang Hyun Choia, Frederick Munb, JaeHwan Leec, Hyunggun Kim*a, Won-Kyo Jung*d, Chul Ho Jang*e and GeunHyung Kim*a
aDepartment of Biomechatronic Engineering, College of Biotechnology and Bioengineering, Sungkyunkwan University, Suwon 440-746, Republic of Korea. E-mail: hkim.bme@skku.edu; gkimbme@skku.edu
bDepartment of Biological Sciences, Carnegie Mellon University, Pittsburgh, USA
cDepartment of Food Science and Biotechnology, Sungkyunkwan University, Suwon 440-746, Republic of Korea
dDepartment of Biomedical Engineering, Pukyong National University, Busan 608-737, Republic of Korea. E-mail: wkjung@pknu.ac.kr
eDepartment of Otolaryngology, Chonnam National University Medical School, Gwangju 500-757, Republic of Korea. E-mail: chulsavio@hanmail.net

Received 13th October 2016 , Accepted 7th December 2016

First published on 12th January 2017


Abstract

In tissue engineering, scaffolds have been widely studied for the purpose of regenerating damaged tissues or organs. Biocompatibility of materials, pore structure, and even growth factors are effective for enhancing cell growth and differentiation. In particular, mammalian collagen is biocompatible and hydrophilic, and provides good cell attachment due to interactions between Arg–Gly–Asp (RGD) domains and cell membranes. However, there have been some limitations on the use of mammalian collagen. In this study, we present a biocomposite scaffold supplemented with collagen extracted from fish skin and phlorotannin from brown algae. The effect of these biocomponents on various physical characteristics, including water wetting ability and tensile properties, was observed. The in vitro cellular activities of the biocomposites were examined using osteoblast-like cells (MG63) to assess cell proliferation and mineralization. The results show that the cells were more highly proliferated on the phlorotannin/fish collagen/alginate biocomposite compared to the control (collagen/alginate). Furthermore, the biocomposite showed significantly higher in vitro calcium deposition (38.37%) and osteogenesis (43.2%), determined by histomorphometric analysis, than the control. Based on these results, the biocomposite supplemented with fish collagen/phlorotannin was demonstrated to be a good potential biomaterial for enhancing bone tissue growth.


1. Introduction

Tissue engineering (TE) is a field in which biomedical scaffolds, cells, and growth factors are combined to regenerate or repair damaged tissues or organs.1 Scaffolds for use in regenerative applications should provide biocompatibility (to prevent adverse response),2 biodegradability (to allow the biomaterial to degrade appropriately as the tissue develops)3 and appropriate mechanical properties (to maintain the structure throughout the regeneration process)4 for successful regeneration of tissues or organs.

In tissue engineering applications, mammalian collagen has attracted attention due to its excellent biocompatibility and ability to promote tissue proliferation and reorganization, inducing various bioactive signals to express specific tissue-related genes.5,6 However, some limitations of collagen as a biomedical material include its relatively poor physical properties (stiffness and strength), disease transmission between different species, immunogenicity, high cost, and even cultural reasons for rejecting animal-derived collagen.5 To overcome the deficiencies of collagen as a biomaterial, several researchers have tried to find new biomaterials that have biological properties similar to those of mammalian-derived collagen,7,8 and have also fabricated various biocomposites that are supplemented with synthetic biopolymers and bioceramics to increase the mechanical properties of pure collagen without losing the biological activities.9–11 Recently, as one of the typical alternatives to mammalian collagen, fish collagen (FC) has been used in tissue engineering applications. It has been reported that FC scaffolds showed outstanding cellular activity in skin regeneration12 and good osteogenesis ability.13 In addition, it is much cheaper, causes a relatively lower immune response, and is completely free from the religious limitations of mammalian collagen.14

In this study, we used collagen from different origins (porcine and fish) to prove that FC can replace porcine-derived collagen for bone tissue regeneration. To achieve this goal, we designed a functional composite scaffold, consisting of microsized poly(ε-caprolactone) (PCL) struts for mechanical support, phlorotannin as a bioactive component, and a collagen/alginate component as a release controller for the coated phlorotannin, as well as a cell-activating component. Especially the collagen/alginate mixture was widely used due to their combination of the efficient encapsulation of growth factor and controllable delivery through rapid gelation of alginate and of the high cell inducement from the collagen component.15–17 It has been shown that in limited amounts, phlorotannin, derived from brown algae (Ecklonia cava), can promote outstanding cellular activities for regenerating bone tissues.18

To fabricate the composite scaffold, an additive manufacturing (AM) technique, which is one of the most attractive fabrication methods to manufacture complex 3D structures, and simple coating method were used. Throughout the fabrication processes, four different PCL-based composite scaffolds were obtained: (a) as a control, PCL mesh-structure coated with collagen/alginate (C/A), (b) PCL mesh-structure coated with phlorotannin (P), (c) PCL mesh-structure coated with phlorotannin and then recoated with collagen/alginate (P/C/A) and (d) PCL mesh structure coated with phlorotannin and then recoated with fish collagen/alginate (P/FC/A). Osteoblast-like cells (MG63) were seeded on the composite scaffolds for in vitro cellular assessment, including live/dead, DAPI/phalloidin, and alizarin red S (ARS) to observe cell proliferation and differentiation. Finally, the scaffolds were used for in vivo study of ectopic bone formation.

2. Experimental

2.1 Materials

PCL (Mw = 45[thin space (1/6-em)]000) was purchased from Sigma-Aldrich (St. Louis, MO, USA). Collagen solution (type I collagen, Matrixen-PSP; Bioland Ltd., South Korea) and fish collagen were prepared at a fixed concentration of 2 wt%. Low-viscosity, high-G-content nonmedical-grade LF10/60 alginate (FMC BioPolymer, Drammen, Norway) was also used at 2 wt%, and a collagen[thin space (1/6-em)]:[thin space (1/6-em)]alginate mixture (1[thin space (1/6-em)]:[thin space (1/6-em)]1) was used to coat the scaffold. Fish collagen was extracted from a flatfish (Paralichthys olivaceus) collected from South Korean seas, and supplied by Prof. W-K Jung (Pukyong National University, South Korea). Detailed isolation and characterization methods have been fully described previously.19 To cross-link the collagen component, it was immersed in a 50 mM 1-ethyl-(3-3-dimethylaminopropyl) carbodiimide hydrochloride (EDC, Mw = 191.7; Sigma-Aldrich) solution in 95% ethanol for 4 h at room temperature, and 5 wt% CaCl2 (Sigma-Aldrich) was used to cross-link the alginate.

The brown seaweed E. cava was collected along the Jeju Island coast of Korea from October 2008 to March 2009. Fresh E. cava was washed three times with tap water to remove salt, epiphytes, and sand attached to the surface of the samples and stored at −20 °C. The frozen samples were lyophilized and homogenized using a grinder before extraction. Phlorotannins were isolated from E. cava powder as described previously by Heo et al.,20 with slight modifications. Briefly, the dried EC powder (500 g) was extracted three times with 80% MeOH and then filtered. The filtrate was evaporated at 40 °C to obtain the methanol extract. Next, the extract was suspended in distilled water and partitioned with ethyl acetate. The ethyl acetate fraction was mixed with celite, dried and packed into a glass column, and eluted in the order of hexane, methylene chloride, diethyl ether, and methanol. The diethyl ether fraction was further purified by Sephadex LH-20 column chromatography using a stepwise gradient chloroform/methanol (2/1 → 0/1) solvent system. The extracted phlorotannin was dissolved in ethanol at 5 wt%. In our previous work, the 5 wt% phlorotannin significantly influenced in vitro bone formation.21

2.2 Fabrication of composite scaffolds

A three-axis robot system supplemented with a melting dispenser can manufacture multi-layered porous PCL structures with constant pore and strut diameters. The pore size, 350 μm, was set for osteoconduction and bone formation through vascularization. As shown in Fig. 1, perpendicular-layered PCL scaffolds (28 × 28 × 1.2 mm) were fabricated using the melt-printing method (temperature = 100 °C, pressure = 500 kPa, nozzle speed = 0.4 mm s−1). After fabrication, the coating process was performed by dipping the PCL scaffold in phlorotannin solution and drying for 24 h. The coated sample was washed five times with distilled water. After drying the scaffold, the weight fraction of phlorotannin in EtOH was measured as 5 wt% for the coated phlorotannin solution. After coating the phlorotannin on the scaffold, it was recoated with either collagen/alginate (C/A) or fish collagen/alginate solution (FC/A).
image file: c6ra25182j-f1.tif
Fig. 1 Schematic representation of the fabrication processes for producing biocomposites containing phlorotannin/fish collagen/alginate.

2.3 Characterizations of the composite scaffolds

The morphology of the scaffolds was visualized by scanning electron microscopy (SEM) (Sirion; FEI, USA). The pore size was defined as the distance between the struts and analyzed using the SEM images.

The water uptake ability was calculated by weighing the scaffolds before and after soaking in distilled water for 12 h. The percentage increase in water absorption was calculated as (%) = (W12 hWo)/A × 100, where W12 h is the weight of scaffolds after 12 h, Wo is the weight at time zero, and A is the area of scaffold.

To observe the biodegradability of the coated component, the initial weight (Wi) of the scaffolds that were only coated with the collagen/alginate or fish-collagen/alginate was measured, and then those were immersed in PBS (pH 7.4) at 37 °C. After incubation for 7 days, the scaffolds were freeze-dried and their weight (Wf) was measured. Because the PCL cannot be degraded for 7 days, we assume the most weight loss was from the collagen/alginate component. The percent weight loss was calculated with the following equation, weight loss (%) = [(WiWf)/Wi] × 100. Weight loss is shown as the mean ± SD of five samples.

Phlorotannin released from the composites was monitored by UV-spectrophotometry (Optizen 2120UVPlus, Mecasys Co., Daejeon, South Korea) in PBS (pH 7.4) at a wavelength of 301 nm. The phlorotannin release test was carried out by incubating the scaffold in 15 mL of PBS solution at 37 °C for various time periods. To measure phlorotannin release, 1 mL of the solution was removed and tested; the aliquot was then returned to the release solution. To avoid contamination of release solution, the pipette tip and cuvette of the spectrophotometer were sterilized with 70% ethanol. The cumulative amount of phlorotannin released was calculated as a function of time.

To assess the mechanical properties, the scaffolds were cut into small strips (5 × 15 mm2). For each 3D scaffold, five samples were taken from different sites. A tensile test was carried out using a tensile machine (Top-tech 2000; Chemilab, South Korea). The stress–strain curves for the scaffolds were recorded at a stretching speed of 0.5 mm s−1. All values are mean ± SD (n = 5).

The fabricated composite scaffolds were immersed in 1× simulated body fluid (SBF), consisting of NaCl (7.995 g), KCl (0.224 g), CaCl2·2H2O (0.368 g), MgCl2·6H2O (0.305 g), K2HPO4 (0.174 g), NaHCO3 (0.349 g), and Na2SO4·10H2O (0.161 g) in 1 L of distilled water. The pH was adjusted to 7.4 by addition of Tris–HCl. The composite scaffolds were added to the fluid and remained there during incubation at 37 °C. After 7 days, the scaffolds were washed with deionized water to remove adsorbed minerals, and lyophilized.

To measure the crystallite size of the biomineralized surface of the fabricated scaffolds, wide-angle X-ray diffraction (WAXD) was performed using a Siemens D 500 WAXD (Siemens, Munich, Germany) with CuKα radiation under beam conditions of 40 kV and 20 mA with spectra collection at 2θ = 5–80° and a step size of 0.1°.

2.4 In vitro cell culture

Fabricated scaffolds (5 × 5 mm2) were sterilized with 70% ethanol and ultraviolet (UV) light. MG63 cells (MG63-human source, ATCC number CRL-1427; ATCC, Manassas, VA, USA) were used to evaluate the behavior of cells cultured in the scaffolds. The cells were cultured for up to nine passages in 24-well plates containing Dulbecco's modified Eagle's medium (DMEM; Hyclone, USA) supplemented with 10% fetal bovine serum (Hyclone) and 1% penicillin–streptomycin (Hyclone). The cells were collected by trypsin-ethylenediaminetetraacetic acid (EDTA) treatment, seeded onto the scaffolds at a density of 1 × 105 per specimen, and incubated at 37 °C in an atmosphere of 5% CO2. The medium was changed every second day.

2.5 Live/dead cell staining

After 1, 3 and 7 days of cell culture, the scaffolds were exposed to 0.15 mM calcein AM and 2 mM ethidium homodimer-1 for 1 h in an incubator to permit observation of live and dead cells. The stained specimens were visualized under a microscope (TE2000-S; Nikon, Tokyo, Japan) with an epifluorescence attachment and a SPOT RT digital camera (SPOT Imaging Solutions, Sterling Heights, MI). Stained images were captured in which green and red indicated live and dead cells, respectively. Image J software (National Institutes of Health, Bethesda, MD) was utilized to enumerate live cells in the width direction of the scaffolds after 7 days of culture.

2.6 DAPI/phalloidin staining

After 7 and 14 days of cell culture, the scaffolds were analyzed with diamidino-2-phenylindole (DAPI; dilution ratio of 1[thin space (1/6-em)]:[thin space (1/6-em)]100, Invitrogen, Carlsbad, CA, USA) staining to characterize the nuclei of the cells. Alexa Fluor 568 Phalloidin (dilution ratio of 1[thin space (1/6-em)]:[thin space (1/6-em)]100, Invitrogen) was used to visualize the actin cytoskeleton of the cells in the scaffolds by fluorescence microscopy (CKX41; Olympus).

2.7 Alizarin red S staining

Calcium mineralization was determined by alizarin red S staining of MG63 cells cultured on the scaffolds in 24-well plates. The cells were washed three times with PBS, fixed in 70% (v/v) cold ethanol (4 °C) for 1 h, and air-dried. The ethanol-fixed specimens were stained with 40 mM alizarin red S (pH 4.2) for 1 h and washed three times with purified water. Specimens were then destained with 10% cetylpyridinium chloride in 10 mM sodium phosphate buffer (pH 7.0) for 30 min. An optical microscope was used to observe the extent of staining, and the OD was measured at 562 nm using a Spectra III UV microplate reader. The OD was normalized to the total protein content (OD value).

2.8 In vivo study for ectopic bone formation

All animal experiments followed a protocol approved by the Committee for Animal Experimentation at Chonnam National University, Korea (CNU IACUC-H-2016-131). We divided fourteen normal (BALB/C) mice into two groups according to the type of scaffold: control group (n = 7, C/A) and study group (n = 7, P/FC/A). General anesthesia was administered by intraperitoneal injection of a mixture of Zoletil (30 mg kg−1; Virbac Lab, Carros, France) and Rompun (10 mg kg−1; Bayer Korea Ltd, Ansan, Korea). Each mouse was shaved at the thigh region and painted with povidone–iodine and ethanol.

Following unilateral posteromedial skin incisions along the right thigh, a muscle pocket was created in each hind limb. The scaffold was inserted into the muscle pocket. After suturing, intramuscular injection of ciprofloxacin was administered.

We harvested thigh muscles containing ectopic bone at 8 weeks after intramuscular implantation to evaluate the histology of the tissues. The round-shaped ectopic bone was isolated after dissection. We carefully detached the muscles and soft tissue affixed to each round ectopic bone mass.

The ectopic bone samples were fixed in 10% formalin solution, decalcified by graded dehydration, and then embedded in paraffin and cut into serial sections with a thickness of 5 mm. The sections were stained with hematoxylin and eosin for examination under a light microscope. Histomorphometric analysis was performed using an image analysis system (Image Inside, Focus Technology, Daejon, Korea).

2.9 Statistical analysis

All data presented are expressed as mean ± SD. Statistical analyses comprised single-factor analyses of variance (ANOVA). The significance level was set at p < 0.05. For in vivo work, the one-way ANOVA test was employed for statistical analysis. The statistical significance was set at 5% and p-values were adjusted for multiple comparisons.

3. Results and discussion

3.1 Micro-/internal structure of scaffold

The optical and SEM images of the fabricated scaffolds are shown in Fig. 2(a–d) and 3(a–d), respectively. In the optical images the yellowish color of the scaffolds (P, P/C/A and P/FC/A) was clearly shown to emphasize the coated phlorotannin component. However, pores of the scaffold (P/C/A) are partly blocked due to the non-homogeneous coating-ability, which is because the porcine collagen could be reacted with tannin component in the phlorotannin.
image file: c6ra25182j-f2.tif
Fig. 2 Optical microscope images of PCL-based biocomposites coated with (a) collagen/alginate (C/A), (b) phlorotannin, (c) phlorotannin/collagen/alginate (P/C/A) and (d) phlorotannin/fish collagen/alginate (P/FC/A).

image file: c6ra25182j-f3.tif
Fig. 3 SEM images of (a) collagen/alginate (C/A), (b) phlorotannin (P), (c) phlorotannin/collagen/alginate (P/C/A) and (d) phlorotannin/fish collagen/alginate (P/FC/A) biocomposites.

It has been shown that the pore size and surface chemistry of biomedical scaffolds directly influence cell adhesion and proliferation.22,23 Generally, it is well known that the appropriate pore size of biomedical scaffolds to induce osteogenic differentiation is between 300 and 500 μm.20 Based on this, we set the pore and strut size of the manufactured scaffolds as 350 μm and 250 μm and, as shown in the surface and cross-sectional optical images, the designed pore structure was well fabricated. We used the SEM images to precisely measure the pore size and observe the surface morphology, and the pore and strut size were found to be about 360 ± 18 μm and 265 ± 21 μm, respectively, confirming that the pore structure was well-fabricated. The surface of the struts was also highly roughened due to the coating components. As expected, the C/A, P/C/A and P/FC/A scaffolds were slightly thicker, due to the mixture of collagen/alginate, than the P scaffold. Using the SEM images, we quantitatively measured the average coated layers of C/A (2 μm), P (0.5 μm), P/C/A (2 μm) and P/FC/A (2 μm thick) on the scaffold surfaces.

3.2 Scaffold characteristics

To observe the in vitro biomineralization ability of the scaffolds, they were immersed in 1 × SBF for 7 days. Fig. 4(a and b) show SEM and energy-dispersive spectroscopy (EDS) images taken before and after in vitro biomineralization of the C/A and P/FC/A scaffolds. In the EDS mapping images, the green and red dots indicate “Ca” and “P”, respectively, and the “Ca/P” ratio on the scaffolds (C/A and P/FC/A) was about 1.65 and 1.53, respectively, which are similar value of hydroxyapatite. As shown in the both SEM images of C/A and P/FC/A scaffold, the mineralized apatite particles are shown. However, the coated region of the collagen/alginate on the surface of the C/A scaffold was not completely homogenous, but the P/FC/A scaffold showed a relatively homogeneously coated surface. It is known that surface roughness homogeneity can directly influence in vitro biomineralization ability, even for surfaces with similar chemical compositions.24 As shown in the SEM image of the C/A scaffold, developed apatite particles were obtained, but the covering was deficient over the whole strut surface (Fig. 4(a)). However, for the P/FC/A scaffold, the apatite particles on the surface were more evenly developed (Fig. 4(b)). This phenomenon could be due to the different coating ability of the coating agents; the fish collagen has a significantly higher solubility in dilute acid and mammalian collagen has lower solubility.14,25
image file: c6ra25182j-f4.tif
Fig. 4 Surface SEM, Ca/P mapping images, and EDS spectra taken before and after in vitro mineralization of (a) collagen/alginate (C/A) and (b) phlorotannin/fish collagen/alginate (P/FC/A) scaffolds. Red arrows indicate the hydroxyapatite particles. (c) X-ray diffraction (XRD) patterns for C/A and P/FC/A.

To quantitatively measure the apatite crystallite size on the strut surface, X-ray diffractometer analysis of the strut surfaces was performed and the results are shown in Fig. 4(c). It is well known that the high diffraction peaks (21.3° and 23.8°) are due to the orthorhombic planes, (110) and (200), of the PCL struts, while the peak (31.8°) was attributed to the crystallite plane, (211), which is generated from the developed hydroxyapatite (HA).26 As shown in the magnified graphs, the peak intensity at 31.8° of the P/FC/A scaffold was significantly higher than that of the scaffold (C/A). In addition, the full-width at half-maximum (FWHM) was measured using the diffracted plane (211) and crystallite size was measured using the Scherer equation, 0.89λ/[β[thin space (1/6-em)]cos(θ)]. In the equation, ‘λ’ is wavelength (0.154 nm), ‘β’ is FWHM, and ‘θ’ is the diffraction angle. The mean size of the crystallites was significantly higher in the P/FC/A scaffold (127 nm) relative to the C/A scaffold (103 nm). The larger crystallite size of the P/FC/A could be due not only to the homogeneously coated FC/A mixture, but also the synergistic effect of the coated phlorotannin component attracting Ca2+, indicating that the scaffold can induce significant osteogenesis to accelerate hard tissue regeneration.

The hydrophilic properties of a scaffold play an important role in promoting cellular activities including initial cell attachment and proliferation.27–29 Therefore, numerous studies have modified the surface chemical composition by coating with biopolymers such as collagen25 and alginate.26 The optical images in Fig. 5(a) show the water wetting of the scaffolds to determine their hydrophilicity. All scaffolds showed outstanding wetting ability due to the hydrophilic coating components (phlorotannin and collagen/alginate). Moreover, the water absorption ability of the scaffolds showed no significant difference (Fig. 5(b)). Based on these results, we confirmed that both the control (C/A) and experimental groups (P, P/C/A and P/FC/A) had sufficient hydrophilic properties to promote initial cellular activities including efficient cell seeding and cell adhesion/spreading.


image file: c6ra25182j-f5.tif
Fig. 5 (a) Transient absorption images of one droplet (5 μL) of water through the cross-section of the scaffolds. (b) Graph comparing water absorption for the various biocomposites (n = 5). (c) Stress–strain curves for the biocomposites and (d) measured moduli. PCL, poly(ε-caprolactone); C/A, collagen/alginate; P, phlorotannin; P/C/A, phlorotannin/collagen/alginate; P/FC/A, phlorotannin/fish collagen/alginate. * indicates p < 0.05 and NS indicates nonsignificance.

The mechanical stiffness of biomedical substitutes should be analogous to those of the environmental tissues to avoid stress-concentration in the affected region, and stiffness can also directly affect cell growth and differentiation.30 Collagen has been used extensively for soft/hard tissue regeneration since it is the main organic component of bone and one of the main components of the extracellular matrix (ECM).31 Although collagen can be considered an ideal component for tissue regeneration, the main weakness of the material is its low mechanical property, so it has been applied in composites and blending systems using biocompatible ceramics and synthetic polymers.9–11 To improve the shortcomings of the collagen/alginate, we used PCL as a structural support. Fig. 5(c) shows the tensile stress–strain curves of the scaffolds with a stretching speed of 0.5 mm s−1. The scaffolds showed a completely similar mechanical behavior, with linear elastic regions and then fluctuating regions due to strain hardening of each strut. As expected, the elastic moduli of the biocomposites were not significantly different (p < 0.05) (Fig. 5(d)).

To observe the biodegradability of the collagen/alginate and fish-collagen/alginate mixtures, weight loss of the scaffolds that were only coated with collagen/alginate (C/A) and fish-collagen/alginate (FC/A) was measured after 7 days in the PBS solution at 37 °C. The degradation of the C/A (5.6 ± 1.2%) and FC/A (6.1 ± 1.6%) scaffolds was similar.

Recently, scaffolds combined with drug delivery systems (DDS) have been widely applied in tissue regeneration.32–34 To effectively regulate the release of biocompatible components, controllable release is required. In our previous works, we investigated the controlled release of various bioactive components, such as fucoidan35 and sulfuretin,36 using a coated alginate to avoid an initial biocomponent burst effect. In this work, we also employed a similar system using the coated collagen/alginate component. Fig. 6 displays the cumulative percent release of phlorotannin from the P, P/C/A and P/FC/A scaffolds. Most of the phlorotannin in the P scaffold without the coating component was released until 1 h. However, phlorotannin release from the P/FC/A scaffold was delayed with the coated component (fish collagen/alginate) and lasted 6–7 days, although 80% of the bioactive component was released in the first 12 h. Based on this result, we can confirm that the fish collagen/alginate layer can delay the phlorotannin release. In addition, as the comparing the release behavior of the P/C/A and P/FC/A, the phlorotannin release of the P/FC/A was meaningfully delayed relative to that of P/C/A. This phenomenon was because of the homogenous coat-ability of the fish collagen/alginate, which was shown in the Fig. 2(d), compared to that of the P/C/A of Fig. 2(c). We can estimate that the bioactive component (phlorotannin) in the P/FC/A scaffold can be continuously released for 7 days. To measure the released amount of phlorotannin at 7 days, we used a standard curve (the optical densities vs. the various concentrations of phlorotannin). By using the curve, we can obtain the total released amount of phlorotannin from the scaffolds (size: 5 × 5 × 1.2 mm3) at 7 days, 2.52 mg (P), 0.59 mg (P/C/A), and 0.53 mg (P/FC/A). The small amount of the coated phlorotannin of the P/C/A and P/FC/A scaffolds was because the more complex cross-linking/washing process was applied during the scaffold fabrication.


image file: c6ra25182j-f6.tif
Fig. 6 Cumulative percent release of phlorotannin from the phlorotannin (P), phlorotannin/collagen/alginate (P/C/A) and phlorotannin/fish collagen/alginate (P/FC/A) biocomposites.

3.3 In vitro tests

To observe in vitro cellular responses to the scaffolds, osteoblast-like cells (MG63) were cultured on them. Cell proliferation is an important factor when evaluating scaffolds because it directly influences successful tissue regeneration. Fig. 7(a) shows the total protein content, indicating proliferated cells, after 7 and 14 days culture periods. To remove the effect of the collagen content of the scaffold, the initial collagen content was measured and subtracted. A significant increase was observed with the P/FC/A and P/C/A scaffold compared to the control, C/A scaffold.
image file: c6ra25182j-f7.tif
Fig. 7 (a) Total protein absorption of the biocomposites after 7 and 14 days of cell culture. (b) Live/dead images after cell culture for 7 days. (c) Cell density after culture periods of 1, 3, and 7 days. (d) DAPI (blue) and phalloidin (red) images after culture for 7 and 14 days on the biocomposites. (e) Number of cells and (f) area fraction of F-actin on the composite scaffolds. * indicates p < 0.05 and NS indicates nonsignificance.

To measure live/dead cells on the scaffolds, they were stained with calcein AM (live) and ethidium homodimer-1 (dead). Fig. 7(b) shows fluorescence images of live (green) and dead (red) cells on the scaffolds after 7 days. Similar to the protein content results, the proliferated live cells were more distributed on the surface of the P/C/A and P/FC/A scaffold compared to the other scaffolds (P and C/A). Using the live/dead images taken after 1, 3, and 7 days, we measured the cell-density for each scaffold (Fig. 7(c)). As expected, the cell-density for the same area was significantly higher in the P/FC/A scaffold. We think this result was due to the synergistic effect of continuously released phlorotannin and the FC/A component facilitating the proliferation of the osteoblast-like cells.

The images in Fig. 7(d) show the nuclei (blue) and F-actin (red) of the proliferated cells on the scaffolds, which were obtained after 7 and 14 days of cell culture. Increased numbers of nuclei and a more developed cytoskeleton were clearly observed in the P/FC/A scaffold, while the control, P, and P/C/A scaffolds showed relatively low activities (Fig. 7(e and f)). This result shows that the P/FC/A scaffold combined with phlorotannin can induce meaningful cellular activities, including cytoskeleton development. Also, as comparing the results of P/C/A and P/FC/A scaffolds, the cytoskeleton activities were more significant in the P/FC/A than those of P/C/A scaffold. We think the relatively low activities of the P/C/A scaffold was occurred due to the non-homogenous coating of collagen/alginate, which was because the porcine collagen was reacted with the phlorotannin.37

In general, calcium deposition results have been used to evaluate the level of calcium mineral in cell culture scaffolds. In Fig. 8(a), optical images of ARS staining of the scaffolds after cell culture for 7 and 14 days are shown. In the images, the red color defines the area of calcium mineral deposition. With increasing culture time, a denser color was observed in all scaffolds. In particular, for the P/C/A and P/FC/A scaffold, the color density was much higher compared to the P and C/A scaffolds, meaning increased calcium mineralization.


image file: c6ra25182j-f8.tif
Fig. 8 (a) Optical images of alizarin red S (ARS) staining of the scaffolds after 7 and 14 days in culture. (b) Relative levels of calcium deposition on biocomposites at 7 and 14 days. * indicates p < 0.05.

The relative optical density (OD) of the red-stained scaffolds, normalized to total protein content, is displayed in Fig. 8(b). The P/FC/A scaffold showed a significantly higher calcium deposition of about 1.4-fold that of the control (C/A scaffold). The result can be attributed to the combined effects of the bioactive component, phlorotannin, and the fish collagen/alginate components promoting osteogenic differentiation of the cells. However, as shown in the result, there is no significant difference of relative calcium deposition between P/FC/A and P/C/A scaffolds.

3.4 In vivo tests

In the in vivo study, we used the scaffolds (C/A and P/FC/A) to observe osteogenesis in the muscle pocket in mice (Fig. 9(a)). The gross appearance showed round-shaped ectopic bone formation in both groups and histological sections showed new bone formation, with the exception of the pores, that are the spaces between the PCL struts. Osteoconduction of the scaffolds was evident in both groups (Fig. 9(b and c)). The control group showed a limited blood vessel network indicated by arrow within the osseous constructs while there were many blood vessels (red arrows) found within the P/FC/A constructs. Histomorphometric analysis showed significantly enhanced osteogenesis with the P/FC/A scaffold compared to the control (Fig. 9(d)).
image file: c6ra25182j-f9.tif
Fig. 9 (a) Subcutaneous implantation of the scaffold (P/FC/A). Histological section showing new bone formation with (b) control (C/A) and (c) phlorotannin/fish collagen/alginate (P/FC/A) scaffolds. The red arrows indicate blood vessels. (d) Histomorphometric analysis. * indicates p < 0.05.

4. Conclusion

In this study, we evaluated the feasibility of fish collagen as a bioactive component to regenerate bone tissue. By employing a combinatorial process of melt-printing/simple coating, the biocomposites consisting of fish collagen/alginate and phlorotannin were fabricated. The construction of biocomposites was a layer-by-layer structure with homogeneous pore size and strut size. The coating agents on the scaffolds provided a good hydrophilic surface and induced meaningful wetting ability. The P/FC/A scaffold showed good in vitro biomineralization in SBF solution compared to the control due to the relatively good solubility of fish collagen. Although the P/C/A using the porcine collagen showed highly efficient to in vitro cellular activities, the newly designed biocomposite (P/FC/A) also showed significantly high cell proliferation and calcium deposition compared to the control (C/A). Through various in vitro and in vivo cellular activities, we have proved that the biocomposite including fish collagen supplemented with phlorotannin can be a potentially significant biomaterial for enhancing bone formation.

Acknowledgements

This study was supported by a grant from the National Research Foundation of Korea grant funded by the Ministry of Education, Science, and Technology (MEST) (Grant no. NRF-2015R1A2A1A15055305), and also supported by grant from Marine Technology Application Program (PJT200673).

References

  1. A. Khademhosseini, R. Langer, J. Borenstein and J. P. Vacanti, Proc. Natl. Acad. Sci. U. S. A., 2006, 103, 2480–2487 CrossRef CAS PubMed.
  2. S. F. Yang, K. F. Leong, Z. H. Du and C. K. Chua, Tissue Eng., 2001, 7, 679–689 CrossRef CAS PubMed.
  3. H. J. Sung, C. Meredith, C. Johnson and Z. S. Galis, Biomaterials, 2004, 25, 5735–5742 CrossRef CAS PubMed.
  4. D. W. Hutmacher, T. Schantz, I. Zein, K. W. Ng, S. H. Teoh and K. C. Tan, J. Biomed. Mater. Res., 2001, 55, 203–216 CrossRef CAS PubMed.
  5. S. Browne, D. I. Zeugolis and A. Pandit, Tissue Eng., Part A, 2013, 19, 1491–1494 CrossRef CAS PubMed.
  6. H. Lee, M. Yeo, S. Ahn, D. O. Kang, C. H. Jang, H. Lee, G. M. Park and G. H. Kim, J. Biomed. Mater. Res., Part B, 2011, 97, 263–270 CrossRef PubMed.
  7. P. Angele, J. Abke, R. Kujat, H. Faltermeier, D. Schumann, M. Nerlich, B. Kinner, C. Englert, Z. Ruszczak, R. Mehrl and R. Mueller, Biomaterials, 2004, 25, 2831–2841 CrossRef CAS PubMed.
  8. G. A. Edwards and G. Roberts, Clin. Mater., 1992, 9, 211–223 CrossRef CAS PubMed.
  9. Y. Hiraoka, Y. Kimura, H. Ueda and Y. Tabata, Tissue Eng., 2003, 9, 1101–1112 CrossRef CAS PubMed.
  10. Y. Kim and G. Kim, J. Mater. Chem. B, 2013, 1, 3185–3194 RSC.
  11. S. Ahn, Y. Kim, H. Lee and G. Kim, J. Mater. Chem., 2012, 22, 15901–15909 RSC.
  12. H. Cao, M. M. Chen, Y. Liu, Y. Y. Liu, Y. Q. Huang, J. H. Wang, J. D. Chen and Q. Q. Zhang, Colloids Surf., B, 2014, 136, 1098–1106 CrossRef PubMed.
  13. J. Elango, J. Y. Zhang, B. Bao, K. Palaniyandi, S. J. Wang, W. H. Wu and J. S. Robinson, Int. J. Biol. Macromol., 2016, 91, 51–59 CrossRef CAS PubMed.
  14. S. Yamada, K. Yamamoto, T. Ikeda, K. Yanagiguchi and Y. Hayashi, BioMed Res. Int., 2014, 2014, 302932 Search PubMed.
  15. H. J. Lee, S. H. Ahn and G. H. Kim, Chem. Mater., 2012, 24, 881–891 CrossRef CAS.
  16. T. A. Becker, D. R. Kipke and T. Brandon, J. Biomed. Mater. Res., 2001, 54, 76–86 CrossRef CAS PubMed.
  17. J. L. Drury and D. J. Mooney, Biomaterials, 2003, 24, 4337–4351 CrossRef CAS PubMed.
  18. B. Ryu, Y. Li, Z. J. Qian, M. M. Kim and S. K. Kim, Chem.-Biol. Interact., 2009, 179, 192–201 CrossRef CAS PubMed.
  19. P. Chandika, S. C. Ko, G. W. Oh, S. Y. Heo, V. T. Nguyen, Y. J. Jeon, B. Lee, C. H. Jang, G. Kim, W. S. Park, W. Chang, I. W. Choi and W. K. Jung, Int. J. Biol. Macromol., 2015, 81, 504–513 CrossRef CAS PubMed.
  20. S. J. Heo, S. C. Ko, S. H. Cha, D. H. Kang, H. S. Park, Y. U. Choi, D. Kim, W. K. Jung and Y. J. Jeon, Toxicol. in Vitro, 2009, 23, 1123–1130 CrossRef CAS PubMed.
  21. M. Yeo, W. K. Jung and G. Kim, J. Mater. Chem., 2012, 22, 3568–3577 RSC.
  22. P. S. Eggli, W. Muller and R. K. Schenk, Clin. Orthop. Relat. Res., 1988, 232, 127–138 CAS.
  23. N. J. Hallab, K. J. Bundy, K. O'Connor, R. L. Moses and J. J. Jacobs, Tissue Eng., 2001, 7, 55–71 CrossRef CAS PubMed.
  24. Y. Kim and G. Kim, Colloids Surf., B, 2015, 125, 181–189 CrossRef CAS PubMed.
  25. P. M. Gallop and S. Seifter, Methods Enzymol., 1963, 6, 635–641 CAS.
  26. S. Koutsopoulos, J. Biomed. Mater. Res., 2002, 62, 600–612 CrossRef CAS PubMed.
  27. K. Rezwan, Q. Z. Chen, J. J. Blaker and A. R. Boccaccini, Biomaterials, 2006, 27, 3413–3431 CrossRef CAS PubMed.
  28. C. H. Lee, A. Singla and Y. Lee, Int. J. Pharm., 2001, 221, 1–22 CrossRef CAS PubMed.
  29. C. H. Jang, S. H. Ahn and G. H. Kim, Int. J. Biol. Macromol., 2016, 10, 1016 Search PubMed.
  30. D. W. Hutmacher, Biomaterials, 2000, 21, 2529–2543 CrossRef CAS PubMed.
  31. J. Glowacki and S. Mizuno, Biopolymers, 2008, 89, 338–344 CrossRef CAS PubMed.
  32. H. Yoon and G. Kim, J. Pharm. Sci., 2011, 100, 424–430 CrossRef CAS PubMed.
  33. Y. Tabata, Tissue Eng., 2003, 9, S5–S15 CrossRef CAS PubMed.
  34. H. H. Sun, T. J. Qu, X. H. Zhang, Q. Yu and F. M. Chen, Biotechnol. Prog., 2012, 28, 3–20 CrossRef CAS PubMed.
  35. G. Jin and G. Kim, Soft Matter, 2012, 8, 6264–6272 RSC.
  36. Y. Koo, H. Lee, S. Kim, N. J. Song, J. M. Ku, J. Lee, C. H. Choi, K. W. Parka and G. Kim, RSC Adv., 2015, 5, 44943–44952 RSC.
  37. F. H. Heijmen, J. S. du Pant, E. Middelkoop, R. W. Kreis and M. J. Hoekstra, Biomaterials, 1997, 18, 749–754 CrossRef CAS PubMed.

This journal is © The Royal Society of Chemistry 2017
Click here to see how this site uses Cookies. View our privacy policy here.