Optimized preparation of micro-block CPAM by response surface methodology and evaluation of dewatering performance

Xiang Liab, Huaili Zheng*ab, Baoyu Gaoc, Yongjun Sund, Xiaomin Tange and Bincheng Xuab
aKey Laboratory of the Three Gorges Reservoir Region's Eco-Environment, State Ministry of Education, Chongqing University, Chongqing 400045, China. E-mail: lx33cqu@163.com; zhl6512@126.com; Fax: +86 23 65120827; Tel: +86 23 65120827
bNational Centre for International Research of Low-carbon and Green Buildings, Chongqing University, Chongqing 400045, China
cShandong Key Laboratory of Water Pollution Control and Resource Reuse, School of Environmental Science and Engineering, Shandong University, Ji'nan 250100, China
dJiangsu Key Laboratory of Industrial Water-Conservation & Emission Reduction, College of Urban Construction, Nanjing Tech University, Nanjing, 211800, China
eChongqing Key Laboratory of Catalysis and Environmental New Materials, College of Environment and Resources, Chongqing Technology and Business University, Chongqing 400067, P. R. China

Received 14th October 2016 , Accepted 3rd November 2016

First published on 22nd December 2016


Abstract

Micro-block cationic polyacrylamide (P(AM-MAPTAC)) was synthesized through UV-initiated template copolymerization and characterized by FTIR, 1H NMR, SEM and TG/DSC analyses. Furthermore, the main influence factors of the preparation process were optimized through Box–Behnken experiment design and Respond Surface Method (RSM). The maximum intrinsic viscosity of micro-block CPAM was 13.223 dL g−1 under the optimum synthesis conditions. The dewatering performance of micro-block CPAM was evaluated taking activated sludge collected from a dyeing mill as the processing object. Results showed that the micro-block CPAM exhibited excellent dewatering performance. At a 30 mg L−1 dosage of micro-block CPAM, the residual turbidity, filter cake moisture content, specific resistance to filtration and chemical oxygen demand removal rate reached 4.47 NTU, 72.2%, 5.47 (1012 m kg−1) and 79.2%, respectively. Dewatering tests not only demonstrated the superiority of micro-block P(AM-MAPTAC) synthesized by UV-initiated template copolymerization over that synthesized by traditional methods but also demonstrated that increasing the molecular weight can further enhance the dewatering performance of flocculants.


Introduction

With the increasing development of the textile industry, dyeing wastewater discharge increases year by year, and a large amount of excess sludge is ultimately produced. Excess sludge disposal has become a major factor restricting the development of the textile industry. Dyeing excess sludge with a high moisture content, complex composition, and high content of harmful substances is categorized as hazardous solid waste.1,2 It is of very important significance to realize a harmless, reduction and stabilization treatment of dyeing excess sludge along with the increase of environmental awareness and strict environmental regulations. In the process of dyeing excess sludge treatment, the moisture content of the concentrated sludge is more than 97%.3 Therefore, dewatering is the most important means of sludge reduction in the whole sludge treatment system. Excess sludge is a colloidal system in which fine sludge particles are suspended in water owing to electrostatic repulsion and is difficult to condense to form a large particle size to facilitate subsequent dewatering process.4,5 Therefore, before the mechanical dewatering, it is necessary to adjust the sludge properties to enhance its dewatering performance.

Cationic polyacrylamide (CPAM) is a kind of synthetic organic compound with excellent sludge dewatering performance.6,7 Positive charged CPAM can effectively neutralize the negative charge on the surface of sludge. Furthermore, long chain molecular structure is conducive to adsorption and bridging effect in the coagulation–flocculation process. Relative molecular weight and cationic degree are considered to be the two most important parameters affecting the flocculation performance of CPAM. Relative molecular weight (limiting viscosity) directly affects the efficiency of bridging effect.8,9 Therefore, to improve the relative molecular weight (MW) of polymer has become an important research direction in CPAM synthesis.10–12 The cationic degree (CD) is closely related to the electrical neutralization performance of CPAM. Besides, CD can also affect the morphology of CPAM in aqueous solution. The strength of the electrostatic repulsion between the positive charges in the CPAM molecular chain can affect the extension of the CPAM molecular chain in water.13–15 However, due to the higher price of the cationic monomer, it is uneconomical to enhance the dewatering performance of CPAM only by increasing the CD. In recent years, researchers have begun to pay attention to the effect of CPAM sequence structure distribution on flocculation performance and some studies have indicated that polymer with cationic micro-block structure is more conducive to the coagulation–flocculation process.16–19 Our previous works have also proved the cationic micro-block structure in CPAM chain is conducive to the electrical neutralization and thus enhance the dewatering performance of CPAM, furthermore, verified the feasibility of synthesizing CPAM with micro-block structure by UV-initiated mode in combination with template polymerization technology.20,21 However, the CPAM with cationic micro-block structure synthesized in our previous works were all with lower molecular weight and thus with a weaker adsorption bridging effect. Therefore, in order to make CPAM play both strong electrical neutralization and adsorption bridging effect in coagulation–flocculation process, it is necessary to optimize the preparation conditions of CPAM to obtain CPAM with both cationic micro-block structure and high relative molecular.

Response surface analysis (RSM) is a statistical method for process design and parameter optimization. In this method, the continuous variable surface model is established to evaluate the factors that affect the reaction process and their interaction, so as to obtain the best experimental conditions. This method has the advantages of short experimental period and can directly reflect the optimal value of the dependent variable, thus received wide attention and extensive application. Hence, this method was used to optimize the synthesis conditions of micro-block CPAM in this study.

In the present study, CPAM with micro-block was synthesized by UV-initiated template polymerization. The properties of micro-block CPAM were tested by using Fourier transform infrared spectroscopy (FTIR), 1H nuclear magnetic resonance (1H NMR), scanning electron microscopy (SEM) and thermal analysis (TG/DSC). Box–Behnken experiment design and Respond Surface Method (RSM) were used to optimize the synthesis conditions of micro-block CPAM. Furthermore, flocculation performance of micro-block CPAM were explored in terms of residual turbidity (RT), filter cake moisture content (FCMC), specific resistance to filtration (SRF), chemical oxygen demand (COD) of supernatant and floc properties.

Materials and methods

Materials

Synthesis reagents. All the reagents used in the synthesis reaction were of analytical reagent grade except acrylamide (AM) and methacrylamido propyl trimethyl ammonium chloride (MAPTAC) (technical grade). The details of the materials are as follows: AM (Chongqing Lanjie Tap Water Company, Chongqing, China); MAPTAC (50 wt% in water; Nanjing Jingruijiuan Biotechnology Co., Ltd. Nanjing, China); EDTA, urea, absolute ethyl alcohol and acetone (Chongqing Chuandong Chemical Industry Co., Ltd. Chongqing, China); VA-044 (Ruihong Biological Technology, Shanghai, China).
Dewatering reagents. All the flocculants used in the dewatering tests were synthesized in our laboratory except the commercial CPAM (technical grade, Chongqing Lanjie Tap Water Company, Chongqing, China). The details of flocculants are listed in Table 1. The dyeing excess sludge was collected from sludge thickener of one dyeing mill in Chongqing China. The sludge featured 99.2% of moisture, 0.95 kg L−1 of density, 10.8 of pH, −16.8 of zeta potential, 8138 mg L−1 of COD and dark green, granular loose and pungent smell of apparent characteristic.
Table 1 Details of flocculants used in dewatering tests
Flocculants Full name of flocculants Intrinsic viscosity dL g−1 Cationic degree (%)
a Flocculants P was synthesized by UV-initiated copolymerization without addition template PAAS.b Flocculants CPAM was commercial product and synthesized taking DAC as the cation monomer.
TP1 Template poly(AM-MAPTAC) 1# 9.050 25
TP2 Template poly(AM-MAPTAC) 2# 11.280 25
TP3 Template poly(AM-MAPTAC) 3# 13.223 25
Pa P(AM-MAPTAC) 13.348 25
CPAMb Commercial P(AM-DAC) 13.386 25


Optimize synthesis conditions by RSM

The synthesis process and characterization methods were described in S1 and S2 Texts. An integrative method of Box–Behnken (BBD) and RSM was used to optimize the synthesis process of micro-block P(AM-MAPTAC), the experimental range for independent variables was preliminary trials based, with negligible error. In the optimization test, five independent variables, pH (X1), concentration of initiator (wt% of total monomer) (X2), mole ratio of PAAS and MAPTAC (n(PAAS/MAPTAC)) (X3), mole ratio of MAPTAC and AM (n(MAPTAC/AM)) (X4), irradiation time (t/min) (X5) were chosen for BBD-RSM approach, while intrinsic viscosity (η/dL g−1) was considered as response variable. The details of BBD experimental design are listed in Table 2. B46 (35) was used to improve the experiment. As given in Table 2, eqn (1) was used to account for the control and prediction of optimization process.
 
image file: c6ra25245a-t1.tif(1)
where β0, βi, βii and βij are regression coefficients, Xi are coded independent variables. The designs contribute to minimize the unexpected effects and set up reasonable mathematical models for optimization process.
Table 2 Levels of the independent variables designed in the B46 (35)
Independent variables Code Levels
−1 0 1
pH X1 3 4.75 6.5
Va-044 (wt%) X2 0.02 0.07 0.12
n(PAAS/MAPTAC) X3 0.5 1 1.5
n(MAPTAC/AM) X4 0.15 0.33 0.5
t (min) X5 30 60 90


Dewatering tests

1 g L−1 (concentration of pure flocculants) of flocculants were pre prepared by dissolving a certain amount of solid flocculants in 100 ml distilled water. All the dewatering tests were conducted on a program-controlled jar-test apparatus (ZR4-6, Zhongrun Water Industry Technology Development Co., China) at room temperature. RT and COD of supernatant, FCMC and SRF of sludge were used to evaluate the dewatering performance of flocculants. In the sludge dewatering test, a set dosage of flocculants was added into 250 ml beaker with 100 ml initial dyeing excess sludge and the pH was adjusted with sodium hydroxide (0.1 mol L−1) and hydrochloric acid (0.1 mol L−1) to the set value. Then quickly stirring at 120 rpm for 20 s and followed by 40 rpm for 60 s, then stand for 10 min. The supernatant 1 cm below the water surface was collected for the measurement of RT, COD and zeta potential, and then the conditioned sludge samples were filtered through a vacuum suction filter machine under a pressure of 0.05 MPa for 30 min for the FCMC and SRF measure. The detail measure methods of RT, COD, zeta potential, FCMC and SRF are described in S3 Text. The sludge settle performance was conducted in a 500 ml graduated cylinder. 500 ml original dyeing sludge with 30 mg L−1 dosage of flocculants was firstly rapid mixed in a beaker and then poured into a 500 ml graduated cylinder. After quickly and repeatedly inverted for 4 times, the height of the solid–liquid surface with time was immediately recorded until the height remained unchanged. Finally, the sludge flocs were collected for size measurement using a laser diffraction instrument (Mastersizer 2000, Malvern, U.K.). The measurement of each sample was repeated conducted for three times, and the average value was taken as the final value for analysis.

Results and discussion

Structure identification

FTIR spectra of polymers. Fig. 1 shows the FTIR spectra of AM, template PAMA (template poly(AM-MAPTAC)) and PMA (poly(MAPTAC)). As shown in Fig. 1 (AM), the absorption peaks at 3354, 1675, 1613, 3189 and 2813 cm−1 were assigned to stretching vibration of N–H, C[double bond, length as m-dash]O and C[double bond, length as m-dash]C; asymmetry stretching vibration of H–C[double bond, length as m-dash] and symmetric stretching vibration of H–C[double bond, length as m-dash].22,23 As shown in Fig. 1 (PMA), the absorption peaks at 3419, 2942, 1634, 1537, 1489, 1480 and 966 cm−1 were assigned to stretching vibration of N–H, –CH3, C[double bond, length as m-dash]O, N–H and methyl groups of quaternary ammonium; deformation vibration of the methylene group in MAPTAC unit and N+ (CH3)3 stretching vibration.24 Comparing with Fig. 1 (AM) and (PMA), as shown in Fig. 1 (template PAMA), the peaks at 3189, 2813 and 1613 cm−1 which represent C[double bond, length as m-dash]C in AM disappeared; the peaks at 2942, 1489, 1480 and 966 cm−1 which represent MAPTAC unit were observed and the peaks at 3354(3419) and 1675(1634) which represent N–H and C[double bond, length as m-dash]O both in AM and MAPTAC unit were also observed. All the corresponding peaks in template PAMA had a certain shift comparing with those in AM and MAPTAC. Therefore, all these characteristic peaks confirmed that the two monomers were successfully copolymerized.
image file: c6ra25245a-f1.tif
Fig. 1 FTIR spectra of polymers.
1H NMR of polymers. The 1H NMR spectra of PMA, template PAMA and PAM are shown in Fig. 2. Comparing with the 1H NMR spectra of PMA and PAM, the corresponding peaks in 1H NMR spectra of template PAMA had a certain shift. The characteristic peaks of H(a′) and H(c) ∼ H(h) at 1.94, 3.66, 2.06, 3.27, 1.77, 3.39 and 3.17 ppm in PMA respectively and the characteristic peaks of H(a) and H(b) at 1.16 and 1.79 ppm in PAM were all observed in the spectra of template PAMA.8,24 The coexistence of characteristic peaks of H(a) and H(a′) resulted from the two link mode of ‘-MAPTAC-AM-’ and ‘-MAPTAC-MAPTAC-’ meanwhile demonstrated the existence of micro-block structure of MAPTAC. Therefore, the results of 1H NMR analysis indicated the successfully copolymerization of AM and MAPTAC moreover the existence of micro-block structure of MAPTAC.
image file: c6ra25245a-f2.tif
Fig. 2 1H NMR spectra of polymers.
SEM of copolymers. The SEM images of template PAMA (5.00k×, 10.00k× and 20.0k×) are shown in Fig. 3. As shown in Fig. 3, template PAMA had a porous structure with a prodigious surface area which could improve its ability of adsorption and bridging. This surface features should owe to the UV initiation mode with surface modification and removal of template PAAS.25,26 Ultraviolet radiation can induce the activation of carbon fiber surface and generation of free radicals. The free radicals react with monomer radicals to form chemical bond thus increased the surface energy and surface roughness (which usually shown as the increase of surface porosity) of carbon fiber. Some existing reports showed that the surface roughness of carbon fiber modified by UV induction mode had been increased which usually shown as the increase of surface porosity. Furthermore, in template PAMA without template separation, the template occupies a certain spatial location. Then with the removal of template, a certain pore formed at the original position of the template, thus porosity of template PAMA was greatly increased. Besides the direct observation of SEM images, the fractal dimension (D) of polymer calculated through image analysis method on the basis of SEM images can also be used to evaluate the surface morphology of polymer.27,28 Fractal dimension which corresponds to the complexity of the system is an important parameter in the study of fractal theory. In this study, Image-Pro Plus 6.0 software had been used to analysis the SEM images of template PAMA and fractal dimension used in this study was two-dimensional fractal dimension defined as double logarithmic relationship of perimeter (L) and projected area (A) of selected region. As shown in Fig. 3, log linear fitting of L and A, the average fractal dimensions of template PAMA was 1.5726 which was much higher than that of polymer flocculants synthesized by conventional method (1.2208, 1.3008, 0.7243, 0.7143) also indicated a highly jumbled surface morphology.
image file: c6ra25245a-f3.tif
Fig. 3 SEM micrographs of template PAMA.
TG/DSC analysis of copolymers. Fig. 4 shows the TG/DSC analysis of template PAMA. As shown in TG curve of Fig. 4. There were three stages of weight loss. Because of the hydrophilic groups in polymer chain, the powder sample was easy to absorb moisture in the air, and as the temperature increased, this part of the moisture began to evaporate. As a result, the strong endothermic peak at the first weight loss stage was observed at about 76.9 °C in the DSC curve, and 13.1% of weight loss was calculated in this stage. The second stage of weight loss was considered for the thermal decomposition of main chemical functional groups such as amide and quaternary ammonium in polymer chain.29 The corresponding endothermic peak at 280.4 °C was observed and 20.7% of weight loss was calculated. Polymer backbone began to thermal decompose at the third stage (311.3–456.3 °C) with a rapid weight loss of 45.1%. Obviously, the two observed endothermic peak at 356.9 °C and 396.0 °C respectively indicated the coexist of two phase structure in the polymer and the existence of MAPTAC micro-block structure was verified from another point of view.20,30
image file: c6ra25245a-f4.tif
Fig. 4 TG/DSC analysis of template PAMA.

Optimize synthesis conditions by RSM

The regression model of intrinsic viscosity affected by pH, concentration of initiator, mole ratio of PAAS and MAPTAC, mole ratio of MAPTAC and AM and irradiation time were calculated using the least square method with the experimental data (S1 Table). The final regression equation in terms of coded factors and the detail of variance analysis of the regression model are shown as eqn (2) and listed in Table 3 respectively. As shown in Table 3, the F-value is 34.35, and p-value (Prob > F) is less than 0.05 indicating statistically significance of this model. At the same time, R2-value of 0.9648 suggested a relatively strong correlation between the observed and predicted values. This model could be used to analyze and predict the optimal conditions for the synthesis of template PAMA by UV-initiated template copolymerization. Furthermore, X1, X2, X4, X5, X1X2, X1X5, X12, X22, X32, X42, X52 were significant model terms, and the order of significant effect were irradiation time (t/min) (X5) > pH (X1) > mole ratio of MAPTAC and AM (X4) > concentration of initiator (X2).
 
[η] = 13.25 + 0.63X1 + 0.57X2 − 0.19X3 + 0.61X4 + 0.81X5 + 0.71X1X2 + 0.33X1X3 + 0.31X1X4 + 0.66X1X5 + 0.096X2X3 + 0.36X2X4 + 0.16X2X5 + 0.31X3X4 + 0.32X3X5 − 0.058X4X5 − 1.52X12 − 1.90X22 − 0.53X32 − 1.00X42 − 2.32X52 (2)
Table 3 Variance analysis of regression model
Source Sum of squares df Mean square F value P value Prob > F  
Model 102.78 20 5.14 34.35 <0.0001 Significant
X1 6.38 1 6.38 42.65 <0.0001  
X2 5.15 1 5.15 34.41 <0.0001  
X3 0.57 1 0.57 3.83 0.0616  
X4 5.92 1 5.92 39.58 <0.0001  
X5 10.48 1 10.48 70.02 <0.0001  
X1X2 2.01 1 2.01 13.42 0.0012  
X1X3 0.42 1 0.42 2.82 0.1053  
X1X4 0.37 1 0.37 2.5 0.1266  
X1X5 1.76 1 1.76 11.73 0.0021  
X2X3 0.037 1 0.037 0.25 0.624  
X2X4 0.51 1 0.51 3.43 0.076  
X2X5 0.11 1 0.11 0.71 0.4059  
X3X4 0.38 1 0.38 2.57 0.1215  
X3X5 0.41 1 0.41 2.71 0.1121  
X4X5 0.013 1 0.013 0.089 0.7677  
X12 20.21 1 20.21 135.06 <0.0001  
X22 31.35 1 31.35 209.53 <0.0001  
X32 2.45 1 2.45 16.36 0.0004  
X42 8.76 1 8.76 58.52 <0.0001  
X52 47.05 1 47.05 314.46 <0.0001  
Residual 3.74 25 0.15      
Lack of fit 3.27 20 0.16 1.74 0.2806 Not significant
Pure error 0.47 5 0.094      
Cor total 106.52 45        


Response surface analysis. Fig. 5 illustrates the interaction effect of X1 (pH) and X2 (concentration of VA-044) ((a) and (c)); X1 (pH) and X5 (irradiation time) ((b) and (d)) on the intrinsic viscosity of polymer. As shown in Fig. 5a, intrinsic viscosity of polymer showed a trend of first increasing and then decreasing along with the increase of concentration of VA-044, and the effect of pH on intrinsic viscosity also showed the same trend. As shown in the contour plot of Fig. 5c, pH showed more significant effect on intrinsic viscosity of polymer than concentration of VA-044, moreover, the interaction between pH and concentration of VA-044 affected the response obviously. Similarly, the effect of irradiation time showed the same trend on intrinsic viscosity of polymer with the concentration of VA-044 (Fig. 5b). However, the irradiation time showed more significant effect on intrinsic viscosity of polymer than pH and the interaction between pH and irradiation time also affected the response obviously. The other 8 interaction effect of factors were no significant indicated from Table 3.
image file: c6ra25245a-f5.tif
Fig. 5 RSM analysis of interaction effect ((a) and (c) interaction effect of X1 (pH) and X2 (concentration of VA-044); (b) and (d) interaction effect of X1 (pH) and X5 (irradiation time)).
Optimization and validation. RSM was used to search for an optimum combination of pH, concentration of initiator, mole ratio of PAAS and MAPTAC, mole ratio of MAPTAC and AM and irradiation time for obtaining polymer with the maximum intrinsic viscosity. The results showed that the predicted intrinsic viscosity of 13.246 dL g−1 would be achieved when the pH, concentration of initiator, mole ratio of PAAS and MAPTAC, mole ratio of MAPTAC and AM and irradiation time were 4.75, 0.07 wt%, 1.0, 0.33 and 60 min, respectively. Five additional independent experiments were carried out under the optimum condition. The predicted value was 13.246 dL g−1 of intrinsic viscosity and the actual experimental mean value was 13.223 dL g−1, indicating that the optimum condition was appropriate.

Dyeing sludge dewatering

Evaluation of dewatering performance. Residual turbidity (RT) of supernatant and filter cake moisture content (FCMC) after flocculation process are the main and direct indicators to evaluate flocculation efficiency of flocculants. Generally, lower RT and FCMC reflect excellent flocculation efficiency. Furthermore, specific resistance to filtration (SRF) is widely used to evaluate the filtration performance of sludge, and lower SRF reflects better dewatering performance of sludge. The effect of flocculants dosage and pH of sludge are illustrated in Fig. 6. As shown in Fig. 6a and b, with the flocculants dosage increased, the RT, FCMC and SRF first decreased to reach the minimum and then increased. This trend was consistent with the typical behavior of polyelectrolyte in the flocculation process reported in the previous literature.31 Furthermore, in the dewatering process of dyeing sludge which featured complex composition, high content of harmful substances, COD of supernatant is also one of the important indicators of concern. Also shown in Fig. 6b, the COD removal rate first increased to the maximum and then slightly decreased along with the increasing of flocculants dosage, this trend was corresponding with the other three indicators. The positively charged flocculants can neutralize the net charge on the surface of the negatively charged sludge, in addition, can reduce the surface tension of water and the thickness of the compressed double layer to reduce the thickness of the water film on the surface of the particle.32 Due to the action of electric neutralization, the colloid particles in the sludge destabilized and gathered, correspondingly, the FCMC, RT and SRF were all decreased. Insufficient of electrical neutralization caused by low dosage of flocculants, electrostatic repulsion and steric effect caused by excess flocculants can cause sludge particles to re stable and not conducive to dewatering.33,34 Comparative analysis of the five flocculants, the TP3 presented the lowest RT, FCMC, SRF (4.47 NTU, 72.2%, 5.47 × 1012 m kg−1) and highest COD removal rate (79.2%) at a lower dosage of 30 mg L−1.
image file: c6ra25245a-f6.tif
Fig. 6 Effect of flocculant dosage and pH of sludge on dewatering performance (experimental condition for a and b: 120 rpm for 20 s, 40 rpm for 60 s, stand for 10 min and pH of 10.0; experimental condition for c and d: 120 rpm for 20 s, 40 rpm for 60 s, stand for 10 min and dosage of TP3, P and CPAM were 30, 40 and 40 mg L−1).

Compare analysis of TP1, TP2 and TP3 which featured the same cationic degree but different intrinsic viscosity, the dewatering efficiency of flocculants derived from the analysis of the indicators were enhanced with the increase of viscosity. This phenomenon indicated that in the sludge conditioning process by this kind of flocculants, bridging effect also played a crucial role. In the process of bridging, the polymer chains can span and reduce the gap between the colloidal particles to make the colloid destabilized and gathered to settle. Polymer with higher intrinsic viscosity feature longer molecular chain, consequently improve the collision probability between flocculants and sludge particle, which is conducive to the trapping and bridging action for colloidal particle.35 Therefore, to improve the intrinsic viscosity of flocculants is one of the important means to enhance the flocculation efficiency. In addition, these results indicated the significance of RSM optimize section in this paper.

In view of the importance of sludge pH in the flocculation process and the pH diversity of sludge to be treated, the study of relationship between the dewatering performance and the pH value of sludge is of great practical significance. The effect of sludge pH on dewatering performance is illustrated in Fig. 6c and d. With the increased pH, after sludge treated by CPAM, the RT, FCMC and SRF sharply decreased to the minimum (13.66 NTU, 82.4% and 12.93 × 1012 m kg−1) at pH 10.0, in addition, the COD removal rate sharply increased to the maximum (67.7%) accordingly. The results indicated that alkaline conditions were more favorable for CPAM to exert flocculation efficiency in the process of dyeing sludge dewatering. However, as shown in Fig. 6c and d, comparing with CPAM, after treated by TP3 and P, the change of the four indicators was slight. This phenomenon could be explained by the high stability of polymer chain of TP3 and P under acid/base condition which could attribute the success to the stable amide bond in the TP3 and P molecular chain instead of acyl oxygen bond in the CPAM molecular chain.

Sludge flocs properties and flocculation mechanism. Sludge settle performance is often regarded as one of the indexes to evaluate the sludge dewatering. Sludge with better settle performance usually has better dewatering performance.36 Generally, flocs size and density in particular, can influence sludge settling performance significantly.37 Fig. 7 SP illustrates the sludge settling behaviors after treated by the five flocculants. Results showed that all the sludge settling had a first fast (within 100 seconds), then slow (within 500 seconds) and steady (within 900 seconds) process. The average sedimentation rates of the fast process were 0.1266, 0.1343, 0.1506, 0.1036 and 0.1124 cm s−1 for TP1, TP2, TP3, P and CPAM respectively. In addition, the final sediment height which indicated the sludge volume after dewatering process were 17.321, 16.430, 14.924, 19.605 and 18.714 cm for TP1, TP2, TP3, P and CPAM respectively. These results indicated that TP3 had the best settle performance among the test flocculants and with the increase of intrinsic viscosity, the settle performance enhanced. In addition, we investigated the flocs size distribution (showed in Fig. 7) which represented another important influence factor of sludge settle performance for the test flocculants. As shown in Fig. 7, the d50 of flocs after treated by the five flocculants was in the following order: TP3 > TP2 > TP1 > CPAM > P. These results also indicated the better settle performance of TP3. Fig. 8 shows the treat effect of TP3 on sludge intuitively. After flocculation process, fine sludge particles formed large and dense flocs and settled to the bottom of the beaker with clarified supernatant. As a result, all the conclusion obtained from flocs properties was in line with the former dewatering performance evaluation indicators.
image file: c6ra25245a-f7.tif
Fig. 7 Sludge floc size distribution at the end of flocculation process and effect of types of flocculants on sludge settling behaviors (experimental condition: dosage of TP1, TP2, TP3, P and CPAM were 40, 40, 30, 40 and 40 mg L−1; pH of 10.0).

image file: c6ra25245a-f8.tif
Fig. 8 Comparison chart before and after flocculation for TP3 (30 mg L−1 of dosage, 10.0 of pH).

Adsorption bridging and charge neutralization are the main mechanism of flocculation process. In addition, zeta potential of flocculation system can verify the charge neutralization effect directly and effectively.38 Fig. 9 illustrates the zeta potential of flocculation system along with the increasing of flocculants dosage. All the zeta potential of system after flocculation process were increased with the increased dosage. This phenomenon indicated charge neutralization played an important role in the flocculation process. Zeta potential of TP1, TP2 and TP3 at their optimum dosage were all close to zero indicated charge neutralization was the mainly flocculation mechanism.39 However, zeta potential of P and CPAM at their optimum dosage were all below zero indicated that charge neutralization played a less important role than that of TP1, TP2 and TP3. Furthermore, TP1, TP2 and TP3 had the almost same of zeta potential which can be considered as the same charge neutralization effect, yet with different dewatering performance. This phenomenon could attribute to the different intrinsic viscosity of polymer which could affect the adsorption bridging effect in flocculation process.


image file: c6ra25245a-f9.tif
Fig. 9 Effect of dosage on zeta potential (experimental condition: dosage of TP1, TP2, TP3, P and CPAM were 40, 40, 30, 40 and 40 mg L−1; pH of 10.0).

Conclusions

In this research, UV-initiated template copolymerization technology was used to prepare cationic polyacrylamide with micro-block structure. All the results of structural characterization verified the successful synthesis and existence of micro-block structure. Furthermore, in order to promote its molecular weight, Box–Behnken experiment design and Respond Surface Method (RSM) were employed to optimum the synthesis conditions taking intrinsic viscosity as the response factor. The optimum synthesis conditions were 4.75 for pH, 0.07 wt% for initiator concentration, 1.0 for mole ratio of PAAS and MAPTAC, 0.33 for mole ratio of MAPTAC and AM, and 60 min for irradiation time respectively, and under these conditions, about 13.223 dL g−1 of intrinsic viscosity can be obtained. Results of dyeing sludge dewatering tests showed that the TP3 with micro-block structure exhibited excellent dewatering performance and at 30 mg L−1 of dosage, and 10.0 of pH, the RT, FCMC, SRF and COD removal rate reached the optimum of 4.47 NTU, 72.2%, 5.47 (1012 m kg−1) and 79.2% respectively; in the range below the optimum intrinsic viscosity obtained in this research, the dewatering performance was promoted along with the increased intrinsic viscosity; TP series of flocculants which synthesized taking MAPTAC as the cation monomer had a wider range of pH application than DAC series of flocculants (CPAM).

Abbreviations

AMAcrylamide
MAPTACMethacrylamido propyl trimethyl ammonium chloride
DACAcryloyloxyethyltrimethylammonium chloride
CPAMCationic polyacrylamide
UVUltraviolet
PAASSodium polyacrylate
VA-0442,2′-Azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride
1H NMR1H nuclear magnetic resonance
FTIRFourier transform-infrared spectroscopy
SEMScanning electron microscopy
TG/DSCThermogravimetric/differential scanning calorimetry
RTResidual turbidity
FCMCFilter cake moisture content
SRFSpecific resistance to filtration
TP(1-3)Template poly(AM-MAPTAC)(1-3)
PPoly(AM-MAPTAC)
CODChemical oxygen demand
RSMResponse surface analysis
MWMolecular weight
CDCationic degree

Acknowledgements

This research was supported by the National Natural Science Foundation of China (Project No. 21477010) and 111 Project (Project No. B13041).

References

  1. H. J. Luo, X. A. Ning, X. J. Liang, Y. F. Feng and J. Y. Liu, Bioresour. Technol., 2013, 139, 330–336 CrossRef CAS PubMed.
  2. X. A. Ning, Y. F. Feng, J. J. Wu, C. M. Chen, Y. J. Wang and J. Sun, et al., J. Environ. Manage., 2015, 162, 81–86 CrossRef CAS PubMed.
  3. H. L. Zheng, Y. J. Sun, C. J. Zhu, J. S. Guo, C. Zhao and Y. Liao, et al., Chem. Eng. J., 2013, 234, 318–326 CrossRef CAS.
  4. J. R. Zhu, H. L. Zheng, Z. Z. Jiang, Z. Zhang, L. W. Liu and Y. J. Sun, Desalin. Water Treat., 2012, 51, 2791–2801 CrossRef.
  5. Y. Qi, K. B. Thapa and A. F. A. Hoadley, Chem. Eng. J., 2011, 171, 373–384 CrossRef CAS.
  6. Y. Liao, H. L. Zheng, L. Qian, Y. J. Sun, L. Dai and W. W. Xue, Ind. Eng. Chem. Res., 2014, 53, 11193–11203 CrossRef CAS.
  7. Y. X. Zhao, B. Y. Gao, Q. B. Qi, Y. Wang, S. Phuntsho and J. H. Kim, et al., J. Hazard. Mater., 2013, 258–259C(6), 84–92 CrossRef PubMed.
  8. H. L. Zheng, Y. J. Sun, J. S. Guo, F. Li, W. Fan and Y. Liao, et al., Ind. Eng. Chem. Res., 2014, 53, 2572–2582 CrossRef CAS.
  9. Y. J. Sun, W. Fan, H. L. Zheng, Y. X. Zhang, F. T. Li and W. Chen, PLoS One, 2015, 10(6), e0130683 Search PubMed.
  10. J. R. Zhu, H. L. Zheng, Z. Z. Jiang, Z. Zhang, L. W. Liu and Y. J. Sun, et al., Desalin. Water Treat., 2013, 51(13–15), 2791–2801 CrossRef CAS.
  11. X. G. Liu, Q. Chen, K. Xu, X. D. Zhang and P. X. J. Wang, Appl. Polym. Sci., 2009, 113(4), 2693–2701 CrossRef CAS.
  12. H. L. Zheng, Y. Liao, M. Z. Zheng, C. J. Zhu, F. Y. Ji and J. Y. Ma, et al., Sci. World J., 2014, 2014, 1–11 Search PubMed.
  13. B. Bolto and J. Gregory, Water Res., 2007, 41, 2301–2324 CrossRef CAS PubMed.
  14. Y. Zhou, G. J. Jameson and G. V. Franks, Colloids Surf., A, 2008, 331(3), 183–194 CrossRef CAS.
  15. Y. Zhou and G. V. Franks, Langmuir, 2006, 22(16), 6775–6786 CrossRef CAS PubMed.
  16. L. J. Wang, G. D. Li, Y. Q. Zhang and H. J. Xiao, Appl. Polym. Sci., 2013, 130(6), 4040–4046 CAS.
  17. W. C. Chai, Y. W. Zhang and Y. F. Hou, Polym. Chem., 2013, 4(4), 1006–1013 RSC.
  18. A. Q. Zhang, Y. H. Shen, X. Y. Zhang, L. C. Han and Z. Z. Wang, J. Polym. Res., 2009, 17(1), 11–17 Search PubMed.
  19. M. Ma and S. Zhu, Colloid Polym. Sci., 1999, 277(2–3), 123–129 CAS.
  20. W. Chen, H. L. Zheng, Q. Q. Guan, H. K. Teng, C. Zhao and C. L. Zhao, Ind. Eng. Chem. Res., 2016, 55, 2892–2902 CrossRef CAS.
  21. Q. Q. Guang, H. L. Zheng, J. Zhai, B. Z. Liu, Y. J. Sun and Y. L. Wang, et al., J. Appl. Polym. Sci., 2015, 132, 41747 CrossRef.
  22. P. Lanthong, R. Nuisin and S. Kiatkamjornwong, Carbohydr. Polym., 2006, 66, 229–245 CrossRef CAS.
  23. N. Şahiner, S. Malcı, Ö. Çelikbıçak, Ö. Kantoğlu and B. Salih, Radiat. Phys. Chem., 2005, 74, 76–85 CrossRef.
  24. A. Pourjavadi, S. M. Fakoorpoor and S. H. Hosseini, Carbohydr. Polym., 2013, 93, 506–511 CrossRef CAS PubMed.
  25. K. H. Hong, N. Liu and G. Sun, Eur. Polym. J., 2009, 45, 2443–2449 CrossRef CAS.
  26. B. Kordoghli, R. Khiari, M. F. Mhenni, F. Sakli and M. N. Belgacem, Appl. Surf. Sci., 2012, 258, 9737–9741 CrossRef CAS.
  27. G. C. Zhu, H. L. Zheng, Z. Zhang, T. Tshukudu, P. Zhang and X. Y. Xiang, Chem. Eng. J., 2011, 178, 50–59 CrossRef CAS.
  28. H. L. Zheng, G. C. Zhu, S. J. Jiang, T. Tshukudu, X. Y. Xiang and P. Zhang, et al., Desalination, 2011, 269, 148–156 CrossRef CAS.
  29. L. Ghimici, I. Dranca, S. Dragan, T. Lupascu and A. Maftuleac, Eur. Polym. J., 2001, 37, 227–231 CrossRef CAS.
  30. Q. Q. Guan, H. L. Zheng, J. J. Zhai, C. Zhao, X. K. Zheng and X. M. Tang, et al., Ind. Eng. Chem. Res., 2014, 53, 5624–5635 CrossRef CAS.
  31. Z. Abdollahi, M. Frounchi and S. S. J. Dadbin, Ind. Eng. Chem., 2011, 17(3), 580–586 CrossRef CAS.
  32. J. P. Wang, S. J. Yuan, Y. Wang and H. Q. Yu, Water Res., 2013, 47(8), 2643–2648 CrossRef CAS PubMed.
  33. Z. Yang, H. Yang, Z. W. Jiang, T. Cai, H. J. Li and H. B. Li, et al., J. Hazard. Mater., 2013, 254, 36–45 CrossRef PubMed.
  34. G. C. Zhu, H. L. Zheng, W. Y. Chen, W. Fan, P. Zhang and T. Tshukudu, Desalination, 2012, 285, 315–323 CrossRef CAS.
  35. M. Hjorth and B. U. Jørgensen, Water Res., 2012, 46(4), 1045–1051 CrossRef CAS PubMed.
  36. Y. G. Chen, Y. S. Chen and G. W. Gu, Chem. Eng. J., 2004, 99, 137–143 CrossRef CAS.
  37. A. R. Heath, P. A. Bahri, P. D. Fawell and J. B. Farrow, AIChE J., 2006, 52(6), 1987–1994 CrossRef.
  38. B. Y. Gao, Y. Wang, Q. Y. Yue, J. C. Wei and Q. Li, Sep. Purif. Technol., 2007, 54, 157–163 CrossRef CAS.
  39. E. Pefferkorn, Adv. Colloid Interface Sci., 2006, 120, 33–45 CrossRef CAS PubMed.

Footnote

Electronic supplementary information (ESI) available. See DOI: 10.1039/c6ra25245a

This journal is © The Royal Society of Chemistry 2017
Click here to see how this site uses Cookies. View our privacy policy here.