First published on 12th January 2017
In recent years, biochar has been well-documented in the literature as a promising soil amendment for the sorption and immobilization of organic contaminants in contaminated soils via its organic functional groups. In this study, original and demineralized cow manure biochars were applied with the aim to evaluate the impact of their mineral component on adsorption and competitive adsorption of oxytetracycline and carbaryl. Adsorption increased greatly for oxytetracycline but decreased slightly for carbaryl after demineralization. Mineral components significantly enhanced overall adsorption of carbaryl but slightly inhibited that of oxytetracycline to biochars, because the dominant sorption mechanisms of oxytetracycline and carbaryl on demineralized biochars were established as pore-filling effects and specific-site sorption, respectively. Competitive adsorption was observed in the binary-solute sorption system, where oxytetracycline outcompeted carbaryl on original biochars, however, carbaryl showed a greater competitive adsorption to oxytetracycline on demineralized biochars. Furthermore, demineralization treatment weakened the competition strength of oxytetracycline to carbaryl but enhanced that of carbaryl to oxytetracycline. This work demonstrated that the demineralization treatment altered the physicochemical properties of biochars and the dominant sorption mechanisms of oxytetracycline and carbaryl, leading to their different changes on competition strength. The results are useful for the application of biochars in the remediation of combined pollution in agricultural soils.
Biochars are carbonaceous materials produced by the pyrolysis of biomass residues from agricultural and forestry production under oxygen-deficient condition.9 Increasingly, these materials are receiving recognition as potential amendments that could help reduce the migration and bioavailability of organic contaminants in soils, thereby reducing their environmental risk.9,10
Owing to their large specific surface area (SSA), and high hydrophobicity and aromaticity, biochars exhibit an extraordinarily strong adsorption affinity for a number of hydrophobic organic contaminants (HOCs).11,12 A better understanding of the sorption characteristics and mechanisms of pesticide and antibiotic onto biochars is essential for effective implementation of biochars as amendments to agricultural soils.
To date, much work has been conducted to investigate the sorption of organic contaminants by biochars. Several recent studies have revealed that the sorption affinity and maximum capacity of biochars for pesticides and antibiotics depended on their degree of carbonization, and surface and bulk properties such as the pore size distribution, specific surface area, hydrophobicity, and polarity.6,11,13,14 In addition, the physicochemical properties of the sorbates (e.g., the molecular weight, hydrophobicity, and polarity) and the solution chemistry conditions (e.g., pH and ionic strength) were also found to play a key role in determining the sorption mechanisms of pesticides and antibiotics by biochars.15–17 Most of these studies have focused on examining the source material from which the biochar was produced and the thermochemical conditions employed in the biochar pyrolysis,6,18,19 as these parameters are known to affect the specific surface area, microporosity, and surface chemistry of biochars. To date, however, investigations directed at examining the impact of the biochar mineral component and its interactions with organic matters of biochars are rather limited in the literature.20–25
The published studies examining the impact of the mineral content of natural soils and carbonaceous materials on the sorption of organic pollutants have focused mainly on single-solute sorption system.6,15,20,21,23–27 The results of these studies have shown that the mineral components and their interactions with the organic matter present in carbonaceous materials exerted a great influence on their overall sorption capacity. On one hand, mineral components can inhibit the non-specific adsorption of organic molecules by blocking access to the pores of carbonaceous materials.15,21,25,28 On the other hand, mineral surfaces can enhance the sorption of polar organic chemicals through site-specific interactions such as electron donor–acceptor and hydrogen-bonding interactions.22,25,29,30 For ionic organic compounds, minerals may provide sites for cation or anion binding interaction.16 Therefore, it seems reasonable to hypothesize that polar pesticide and ionic antibiotic could be capable of forming strong complexes with (i) the hydroxyl groups of inorganic silicates and other minerals, and (ii) the electron-rich aromatic structures of organic components (e.g., graphite surfaces) associated with biochars. Combined together, the mineral components of biochars and their interactions with organic moieties are expected to influence the overall sorption characteristics of pesticides and antibiotics on biochars. However, studies examining the impact of mineral content of biochars on the overall adsorption and competitive adsorption of co-existing pesticides and antibiotics are extremely scarce.
Biochars derived from livestock manure usually possess a high mineral content,6,15,19 for this reason, we employed cow manure biochars as the adsorbents in this study. A carbamate insecticide (carbaryl) and a tetracycline antibiotic (oxytetracycline) were selected as a model pesticide and antibiotic, respectively. These compounds have been selected in particular because they have been widely detected in the surface water and in agricultural soil.31,32 The adsorption of carbaryl and oxytetracycline on original and demineralized biochars in single- and binary-solute systems were investigated and the main adsorption mechanisms were discussed. The objectives of this study are to evaluate the impact of mineral components in biochars on the adsorption and competitive adsorption of a pesticide and an antibiotic, and thus develop a better understanding of their sorption mechanisms. The obtained results are expected to provide a firm theoretical groundwork for further analyses of the potential application of biochars in the remediation of combined pollution in agricultural soils.
a Values obtained from Ji et al.20 and Zhang et al.15b MW, molecular weight.c Sw, solubility in water (in mg L−1), data from Marie et al.39d Kow, octanol–water partition coefficient, data from Kulshrestha et al.29 and USEPA.40e pKa, acid dissociation constant, data from Kulshrestha et al.29 | ||
---|---|---|
Compound | OTC | CBL |
Structure and sizea | ||
Formula | C22H24N2O9 | C12H11NO2 |
MWb | 460.43 | 201.22 |
Sw (mg L−1)c | — | 82.6 |
Kowd | 0.11–0.34 | 2.36 |
pKae | 3.27, 7.32, 9.11 | — |
Cow manure stock was collected from a hoggery in Longyou County, Zhejiang, China. The samples were air-dried, ground, passed through a 2 mm sieve, and pyrolyzed in a preheated muffle furnace at either 300, 400, 500, 600, or 700 °C for 6 h under oxygen-deficient conditions as described by Zhu et al.11 The prepared biochars were referred to as CMBCX, where CMBC referred to the cow manure-derived biochar, and X referred to the pyrolysis temperature. The produced biochars were ground and passed through 200-mesh sieve and stored in amber glass bottles at room temperature for later use.
Demineralized biochars were prepared using the method described by Yang et al.33 for elimination of inorganic components. Briefly, the original biochars CMBC600 and CMBC700 were first treated by repeated rinsing with aqueous HCl (1 M), followed by rinsing with a mixture of aqueous HCl (1 M) and HF (1 M), and lastly, by rinsing with distilled water several times until solution pH was neutral, in order to remove any residual acid and soluble salts. The resulting products were freeze-dried and stored in desiccators for later use. Using the original notation based on the pyrolysis temperature, these demineralized biochar samples were referred to as DCMBC600 and DCMBC700, where D denotes demineralized. The prepared biochars were characterized by bulk elemental compositions analysis and surface elemental compositions analysis using an elemental analyzer (Thermo Finnigan Flash EA 1112), and X-ray photoelectron spectroscopy (XPS) (ULVAC-PHI PHI 5000 VersaProbeII, Japan). The ash content of biochars was measured by determining the residual weight after the biochars were heated at 900 °C for 4 h. The oxygen content was calculated by mass difference. The surface area, pore volume, and identity of surface functional groups were characterized using the Brunauer–Emmett–Teller (BET) analysis, and Fourier-transform infrared spectroscopy (FTIR).
In single-solute sorption experiments, the initial aqueous concentrations of OTC and CBL were 4–40 mg L−1 and 8–80 mg L−1, respectively. Binary-solute sorption experiments were conducted on CMBC600 and CMBC700, and the corresponding demineralized biochars DCMBC600 and DCMBC700. In these experiments, OTC or CBL was selected as the primary sorbate (4–40 mg L−1 concentration range), with CBL or OTC as the co-sorbate at a fixed concentration of 32 mg L−1.
The isotherm data obtained in this study were fitted to the Freundlich model adsorption as described by eqn (1) or (2):
Qe = KFCen, | (1) |
logQe = logKF + nlogCe, | (2) |
Sorbent | Bulk elemental compositiona (%) | Atomic ratioc | SBETd (m2 g−1) | Vte (cm3 g−1) | Vmicf (cm3 g−1) | |||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|
C | H | N | O | fomb | Ash | H/C | O/C | (O + N)/C | ||||
a Determined using an elemental analyzer.b Organic matter content.c Calculated from the atomic ratio of the bulk elements.d Determined by N2 adsorption using the Brunauer–Emmett–Teller (BET) method.e Total pore volume, determined at P/P0 = 0.99.f Micropore volume, calculated using the t-plot method.41 | ||||||||||||
CMBC300 | 45.7 | 3.2 | 2.6 | 17.3 | 65.2 | 34.8 | 0.84 | 0.28 | 0.33 | 8.8 | 0.029 | 0.000 |
CMBC400 | 45.3 | 2.6 | 2.3 | 14.5 | 57.7 | 42.3 | 0.69 | 0.24 | 0.28 | 15.2 | 0.03 | 0.000 |
CMBC500 | 42.5 | 1.5 | 2.1 | 11.5 | 50.9 | 49.1 | 0.42 | 0.20 | 0.24 | 21.1 | 0.038 | 0.006 |
CMBC600 | 44.3 | 1.1 | 2.0 | 8.1 | 47.5 | 52.5 | 0.29 | 0.14 | 0.18 | 81.4 | 0.061 | 0.036 |
CMBC700 | 41.8 | 0.6 | 1.2 | 6.7 | 45.8 | 54.2 | 0.18 | 0.12 | 0.15 | 161.4 | 0.11 | 0.074 |
DCMBC600 | 49.2 | 1.7 | 1.0 | 43.6 | 95.4 | 4.6 | 0.40 | 0.67 | 0.68 | 246.6 | 0.20 | 0.090 |
DCMBC700 | 49.5 | 1.3 | 1.0 | 40.5 | 92.2 | 7.8 | 0.31 | 0.61 | 0.63 | 321.3 | 0.26 | 0.12 |
The demineralization treatment of CMBC600 and CMBC700 resulted in essentially complete removal of the mineral components (Table 2). The surface elemental compositions as determined by XPS and surface atomic ratios of the prepared biochars are presented in Table S1.† Carbon was found to be the dominant surface element, followed by oxygen. The main mineral element present on the surface of these biochars was Si. The content of most surface elements decreased, with the exception of C and N, while most mineral elements could even not be detected at all. The surface C content of original CMBCs was obviously higher than their corresponding bulk C, suggesting the minerals of these original biochars were likely covered by organic component as well as the structural heterogeneity within biochars as reported by Zhang et al.15 and Sun et al.21 Furthermore, the increased surface C contents of the CMBCs after demineralization was consistent with their increased bulk C amounts (Tables 2 and S1†), suggesting that minerals of these CMBCs had no obvious effect on the spatial distribution of organic matter, which is not consisted with the result reported by Sun et al.21
The demineralization treatment also decreased the bulk aromaticity and hydrophobicity, while at the same time increased the bulk polarity of the original biochars, as indicated by the increasing atomic ratios of H/C, O/C, and [(O + N)/C] in the demineralized biochars (Table 2). The FTIR spectra can also verify the result mentioned above (Fig. S1†). However, the surface hydrophobicity of original biochars was found to increase while the surface polarity decreased after demineralization treatment (Table S1†), which was a trend opposite to that observed for the bulk properties. This difference in properties suggests that abundant minerals of biochars would benefit the exposure of polar groups on the surface of the tested biochars, which could exhibit higher surface polarity of original biochars than their corresponding demineralized ones.21
The surface area and the pore volume of all biochars were found to increase with increasing pyrolysis temperature, and a particularly large difference was observed for the biochars produced at the highest temperature (Table 2). For CMBC600 and CMBC700, the micropore volumes accounted for a significant proportion (58–69%) of the total pore volumes (Fig. S2†). After demineralization, the surface area and the micropore volume of biochars increased much more significantly, with the greatest change observed for DCMBC700. However, the percentage of the micropore volume in the total pore volume decreased to 44–47% for DCMBC600–DCMBC700 because of the increase in their mesopore volume.
Fig. 1 Adsorption isotherms of oxytetracycline (OTC) and carbaryl (CBL) on original biochars pyrolyzed at different temperatures (300–700 °C). |
According to the results presented above, CMBCs derived at different temperatures displayed dissimilar sorption characteristics for OTC and CBL. To further elucidate the factors that govern the adsorption of OTC and CBL on CMBCs, the chemical structural parameters of these biochars were correlated with the organic carbon-normalized sorption coefficient (logKoc values at three different sorbate concentrations, Table S2†) and the nonlinearity index (n values, Table S2†) of OTC and CBL (Fig. S3 and S4†). This comparison showed that the logKoc values of OTC and CBL at all three different sorbate concentrations were significantly negatively correlated with the H/C, O/C, and [(O + N)/C] atomic ratios of the original biochars, revealing the positive effect of the aromatic and hydrophobic carbon contents of biochars and the negative effect of their bulk polarity on the OTC and CBL adsorption. These observations are in agreement with the findings presented in recent studies,15,20,36 which have shown that OTC and CBL can interact strongly with the aromatic surfaces of carbonaceous adsorbents via strong π–π electron donor–acceptor (EDA) interactions. Additionally, it has been well-documented in literatures11,37 that the adsorption of HOCs to carbonaceous adsorbents can be inhibited by surface polar oxygen-containing functional groups because these groups can facilitate formation of larger and denser water molecule clusters around them, and in turn, creates a stronger competition for the surface area available on the graphitized carbon of adsorbents. Hence, in the present study, the decrease in the H/C and O/C atomic ratios of the original biochars is expected to enhance the π–π EDA interactions, contributing to the sorption of OTC and CBL. Additionally, the aromaticity of CMBCs in this study was higher than the aromaticity of biochars examined in the prior sorption study for OTC and CBL,8,17 and thus, the CMBCs showed a higher sorption affinity for both OTC and CBL.
Fig. S4† clearly shows that the values of n in the CBL sorption isotherms on the original CMBCs were significantly positively correlated with the H/C, [(O + N)/C], and O/C atomic ratios, but no significant correlation was found between the n values in the OTC sorption isotherms and the chemical structure parameters of the original biochars. Therefore, the increase in the aromatic and hydrophobic organic components in the CMBCs with an increasing pyrolysis temperature is the major factor contributing to the nonlinearity of the CBL sorption isotherms, which can provide specific sorption sites for π–π EDA interactions and hydrophobic effect. Although no significant correlation was found between the values of n for OTC and the chemical structural properties of the original biochars, the n values of OTC were markedly lower than those of CBL. This difference suggests that pore-filling at the limited surface and/or interior sites may be the dominant mechanism for OTC adsorption.35 In comparison to CBL, OTC is a much larger molecule (1.41 nm versus 0.71 nm, see Table 1), and it may, therefore, experience pronounced steric hindrance when approaching the sorption domains in the micropores, resulting in a weaker sorption affinity than that of CBL.
Sorbent | Competitor | logKF | n | R2 | logKoca at | |||
---|---|---|---|---|---|---|---|---|
Ce1b | Ce2b | Ce3b | ||||||
a Koc is the concentration-dependent organic carbon-normalized sorption distribution coefficient (Koc = KFCen−1/foc), in L kg−1 of organic carbon, where foc is the percentage of carbon content of biochar.b For OTC, Ce1, Ce2, and Ce3 were 0.2, 2.0, and 20 mg L−1, respectively. For CBL, Ce1, Ce2, and Ce3 equaled to 0.005Sw, 0.05Sw, and 0.5Sw, respectively. Sw (mg L−1) is the solubility of carbaryl in water under neutral pH. | ||||||||
OTC | CMBC600 | — | 3.59 | 0.323 | 0.969 | 4.499 | 3.822 | 3.145 |
32 mg L−1 CBL | 3.48 | 0.364 | 0.964 | 4.361 | 3.725 | 3.089 | ||
CMBC700 | — | 3.77 | 0.395 | 0.978 | 4.646 | 4.041 | 3.436 | |
32 mg L−1 CBL | 3.76 | 0.428 | 0.923 | 4.683 | 4.011 | 3.339 | ||
DCMBC600 | — | 4.15 | 0.171 | 0.989 | 5.038 | 4.209 | 3.380 | |
32 mg L−1 CBL | 3.87 | 0.338 | 0.995 | 4.641 | 3.979 | 3.317 | ||
DCMBC700 | — | 4.42 | 0.164 | 0.983 | 5.309 | 4.473 | 3.637 | |
32 mg L−1 CBL | 4.25 | 0.254 | 0.981 | 5.076 | 4.330 | 3.584 | ||
CBL | CMBC600 | — | 4.11 | 0.382 | 0.973 | 4.783 | 4.165 | 3.547 |
32 mg L−1 OTC | 3.60 | 0.845 | 0.995 | 4.096 | 3.941 | 3.786 | ||
CMBC700 | — | 4.43 | 0.282 | 0.887 | 5.159 | 4.441 | 3.723 | |
32 mg L−1 OTC | 3.98 | 0.667 | 0.976 | 4.561 | 4.228 | 3.895 | ||
DCMBC600 | — | 4.02 | 0.213 | 0.997 | 4.630 | 3.843 | 3.056 | |
32 mg L−1 OTC | 3.92 | 0.268 | 0.990 | 4.509 | 3.777 | 3.045 | ||
DCMBC700 | — | 4.37 | 0.162 | 0.989 | 4.997 | 4.159 | 3.321 | |
32 mg L−1 OTC | 4.25 | 0.223 | 0.997 | 4.853 | 4.076 | 3.299 |
The demineralization treatment removed the majority of the mineral components and created a large number of additional micropores on the biochars, which possess a wide distribution of sorption site energies and can increase the degree of isotherm nonlinearity.21,35 Therefore, demineralization may enhance the site-specific interactions and pore-filling on the biochars and give rise to the significantly nonlinear adsorption of OTC and CBL. This sorption enhancement, however, could be somewhat counteracted by the contributions of the mineral components—it is well documented in the literature that tetracyclines can adsorb strongly on the surfaces of iron/aluminum hydroxides and clay minerals via surface complexation (e.g., mediated by H-bonding) and/or ion exchange reactions.29,30 Furthermore, studies have shown that clay minerals can adsorb CBL through site-specific interactions between the carbamate functional groups and the exchangeable cations present on the mineral surface.26
In order to determine the impact of the mineral components in the original biochars on its overall adsorption of OTC and CBL, the measured adsorption isotherms for the demineralized biochars were fractionalized according to the content of organic matter of the original biochars. The corresponding Freundlich fitting curves (estimated isotherms) are also shown in Fig. 2, representing the adsorption capacity of the organic matter fraction in the original biochars. The differences between the measured and the estimated sorption isotherms represent the minimum adsorption contribution or adsorption inhibition of the mineral fraction. For OTC, the estimated isotherms were located slightly above the measured isotherms, with differences of less than 25% for CMBC700, and less than 15% for CMBC600. However, these trends were completely reversed for CBL, as showed in Fig. 2. Namely, the estimated CBL isotherms were placed well below the measured isotherms for both CMBC600 and CMBC700, with a difference of more than 50% in each case. Based on the comparison of the estimated and the measured sorption isotherms for OTC and CBL, it can be established that the mineral components inhibit slightly the overall sorption of OTC to the original biochars, and enhance significantly the sorption of CBL. However, this observation is not consistent with previously reported studies,15,20 in which the mineral content was found to have a negative influence on the overall adsorption of CBL to biochars, and a significant positive contribution for tetracycline adsorption to black carbon. This discrepancy could be attributed to the differences in the main mechanisms of adsorption of OTC and CBL on the demineralized biochars.
The demineralization treatment decreased the bulk aromaticity and hydrophobicity of biochars but increased their bulk polarity, while the logKoc of OTC still increased significantly, which means that it is not the site-specific sorption mechanism but another sorption mechanism that contributed to the OTC sorption the most. The demineralization process removed most of the mineral content of CMBC600 and CMBC700, thereby reducing the contribution of the mineral components to the adsorption of OTC. However, the demineralization simultaneously released a large number of additional surface micropore sorption sites as pores and surface areas drastically increased, thereby enhancing the accessibility of the sorption sites and pore-filling effect for the adsorption of OTC. Namely, the increase in the logKoc values and the decrease in the values of n (well lower than 1) for the OTC sorption isotherms on the demineralized biochars, together with the increased surface area and the number of pores are indicative of the pore-filling mechanism. In addition, the surface oxygen content of the demineralized biochars was found to be notably lower than that of the original biochars (see Table S1†). Therefore, the demineralization treatment would be expected to reduce water molecule clusters competition adsorption mentioned above. Hydrogen-bonding interactions between the OTC and the biochars might also be enhanced6 following demineralization because the content of certain polar groups increased, as evidenced by the changes in the [O + N]/C atomic ratio and the results of the FTIR spectroscopy analysis. The sorption enhancements mentioned above could counterbalance the loss of mineral contents sorption induced by demineralization, and potentially even can increase the overall adsorption of OTC. Nevertheless, while the number of micropores and the surface area increased significantly after demineralization, the π–π EDA and ion exchange interactions between CBL and biochars may be reduced as a result of the decrease in the aromatic and mineral content, thus actually leading to an overall decrease in adsorption. Hence, it is hypothesized that the main mechanism of OTC sorption on the demineralized biochars is the pore-filling effect, whereas the CBL adsorption can be attributed to the specific site adsorption such as π–π EDA interactions.
Fig. S2† shows the results of the pore size distribution analysis. While the demineralized biochars were found to be highly microporous, the ratio of micropore volume to the total pore volume was lower compared to that of original biochars. This difference can be attributed to the increase in the mesopore volume following demineralization. Meanwhile, the two examined sorbates vary significantly in molecular size, and thus, may exhibit size-dependent adsorption on the selected biochars, regulated by the porosity of the adsorbent. To test this hypothesis, the adsorbent surface area-normalized adsorption isotherms of OTC and CBL on two original and two demineralized biochars are shown in Fig. 3. Comparison of the original sorption isotherms (Fig. 2) and the adsorbent surface area-normalized adsorption isotherms (Fig. 3) reveals that the differences in the adsorption affinities between the original and demineralized biochars for OTC are significantly larger in the original sorption isotherms than in the surface area-normalization sorption isotherms. This outcome indicates that the higher adsorption affinity of the demineralized biochars for OTC than that of the original ones can be largely attributed to their larger surface area and mesopore volume, and further confirms the pore-filling effect as the main sorption mechanism for OTC on demineralized biochars. In contrast, the differences in the adsorption affinities for CBL between the original and demineralized biochars are much more noticeable in the surface area-normalized isotherms than that in the original isotherms. This means that it is not the increase in the biochar surface area that plays a key role in the decrease of the adsorption affinity for CBL but other factors induced by the demineralization process. These results have demonstrated that the sorption of OTC and CBL on demineralized biochars proceeds through different mechanisms.
Fig. 3 Adsorbent surface area-normalized adsorption isotherms for oxytetracycline (OTC) and carbaryl (CBL) on original (CMBCs) and demineralized (DCMBCs) biochars. |
Fig. 4 Adsorption isotherms of carbaryl (CBL) and oxytetracycline (OTC) on original (CMBCs) and demineralized (DCMBCs) biochars with and without a co-solute ([OTC] or [CBL] = 32 mg L−1). |
The strength of the competitive adsorption can be evaluated with a parameter A,38 which expresses the percentage decrease in Koc following the addition of the co-solute and can be calculated using eqn (3):
A = (Koc − K′oc)/Koc × 100%, | (3) |
The values of n determined in the CBL sorption isotherms on original biochars in the presence of OTC increased significantly (from 0.382 to 0.845 for CMBC600, and from 0.282 to 0.667 for CMBC700, Table 3). In contrast, there was little change in the values of n for OTC with CBL as the co-solute, implying that OTC can occupy and block certain sorption sites specific for CBL.30 For this reason, OTC showed stronger competitiveness relative to CBL on CMBC600 and CMBC700. After demineralization, the changes in the values of n in the CBL sorption isotherms with OTC as the co-solute were not as significant as those determined for OTC with CBL as the co-solute. A possible explanation for this observation is that the high-energy sorption sites offered by micropores are preferentially occupied by the smaller adsorbates (CBL).20 We have established that the main sorption mechanism for OTC on demineralized biochars is pore-filling. Therefore, CBL can occupy the micropores on demineralized biochars preferentially inducing a strong size-exclusion effect for the larger OTC molecules. Clearly, demineralization treatment changed the physicochemical properties of biochars and in turn altered the main sorption mechanisms for OTC and CBL on these materials, leading to changes in the competitiveness of OTC and CBL for binding sites. This observation, however, is not consistent with the sorption affinities—the values of logKoc for the CBL sorption isotherms were higher than those for the OTC on the original biochars, but at the same time lower than those of OTC on the demineralized biochars. In other words, a higher sorption does not always lead to a stronger competition. This phenomenon has also been observed in the study of Wang et al.,38 where the sorption coefficients of sulfamethoxazole on activated carbon were found to be larger than those of sulfamethoxazole on single-walled carbon nanotubes. Yet, the sorption competition strength of sulfamethoxazole to carbamazepine was weaker on activated carbon than on single-walled carbon nanotubes in this study.
The results also reveal that the demineralization treatment weakened the competition strength of OTC to CBL, but enhanced that of CBL to OTC. As it can be seen from Fig. 5 that the values of A for the competition of OTC to CBL on original biochars were 2.23–2.86 fold higher than those determined on the demineralized biochars. In contrast, the A values of CBL to OTC on the original biochars were 2.06–4.19 fold lower than those determined for the demineralized biochars. This observation can be attributed to the different main mechanisms for the adsorption of OTC and CBL on demineralized biochars that we have established above. The sharp increase in SSA and the number of pore structures on the demineralized biochars offered abundant specific sites for CBL adsorption, thereby weakening the competitiveness of OTC to CBL following the demineralization treatment. Furthermore, as a result of its smaller size relative to OTC, CBL can take priority over OTC in occupying the micropores available on the demineralized biochars, and then markedly reduced the pore-filling effect of OTC. Ultimately, this phenomenon explains the greater competitiveness of CBL to OTC on demineralized biochars.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c6ra26534k |
This journal is © The Royal Society of Chemistry 2017 |