Qin Wu,
Chen Liu,
Jinjun Peng and
Fujian Liu*
College of Chemistry & Chemical Engineering, Shaoxing University, Shaoxing, Zhejiang 312000, China. E-mail: fjliu@usx.edu.cn
First published on 3rd April 2017
Visible-light active, carbon doped and ordered mesoporous SiO2–TiO2 nanocomposites (C-OMS@TiO2-xs) were synthesized from the self-assembly of Si and Ti precursors with block copolymer templates (F127 and P123), hydrothermally treated at 180 °C, and calcination or extraction for removing the templates. XRD patterns and TEM images indicate highly ordered mesopores were formed in C-OMS@TiO2-xs, and TiO2 species with a high crystalline degree were homogeneously dispersed into the samples, which formed a stable “brick-and-mortar” nanostructure. N2 adsorption–desorption isotherms indicate very large BET surface areas (224–553 m2 g−1) and pore volumes (0.45–1.4 cm3 g−1) in these samples. EDX spectra and elemental maps further confirm successful doping and homogeneous dispersion of TiO2 nanocrystals in C-OMS@TiO2-xs. XPS spectra confirmed the doping of carbon atoms into the lattice of TiO2 species under high temperature hydrothermal conditions, which results in C-OMS@TiO2-xs with enhanced visible light response properties, as confirmed by UV-vis diffuse reflectance spectra and photocurrent–time (I–t) curves. Catalytic tests indicate that the synthesized C-OMS@TiO2-xs show excellent activities for degradation of organic pollutants irradiated with visible light. For instance, degradation of highly concentrated rhodamine B (RhB, 100 ppm) can be completely catalyzed in the water within 50 min. This work provides a facile approach to the targeted synthesis of visible active and ordered mesoporous materials.
One of the most important applications of TiO2 based materials is photocatalysis. However, TiO2 is only sensitive to UV-light due to its large band gap (3.2 eV) in nature, which must be excited by UV-light. However, UV-light accounts for rather limited content of solar radiation energy.22–24 Therefore, extended photocatalytic response of traditional TiO2 materials into visible light region and properly reduce charge-carrier recombination rate would greatly promote their practical applications.22–28 Up to now, several methods have been used to decrease the band gap energy of TiO2, including defects generation by H2 reduction,29–31 doping by transition metal32,33 and nonmetallic ions (S, N, C etc.) into TiO2 lattice.33–35 However, the reported modification processes were usually performed under rather complicated or harsh conditions.27,32–37 Meanwhile, the reported visible light active TiO2 based photocatalysts usually show poor porosity or nanocrystalline morphology, which lead to the drawbacks such as low exposure degree of catalytically active sites, easily sintering and complicated separation processes from the reaction mixtures.2,8,21,31–36
The preparation of mesoporous TiO2 monolith with micrometer sizes could overcome the above problems. However, the mesostructures collapse and lose most of the porosity after being heated up to 300–350 °C because of the intrinsical crystallization of anatase phase.2,21,38–40 An alternative way is to immobilize TiO2 nanocrystals into ordered mesoporous materials, which usually show enhanced stability of mesostructures at high temperatures.2,21,37 Notably, ordered mesoporous materials show unique structural characteristics including controllable morphology, large BET surface areas, versatile frameworks, ordered and uniform mesopores, which strongly enhance the accessibility of catalytically active sites and simplify their regeneration processes.2,21,37,41–43 For instance, Zhao and coworkers successfully immobilized active TiO2 nanocrystals onto the networks of ordered mesoporous TiO2 and carbon, which showed much improved photocatalytic activities for degradation of organic dyes in comparison with commercial P25 irradiated with UV-light.2,21 However, it remains a challenge to synthesize ordered mesoporous TiO2 based photocatalysts with visible-light response.
In this work, we innovatively developed high temperature (180 °C) hydrothermal technology to the synthesis of carbon doped, ordered mesoporous SiO2–TiO2 nanocomposites (C-OMS@TiO2-xs), the ordered mesostructure was formed from self assembly of block copolymer templates with Si, Ti precursors. Interestingly, the unique high temperature (180 °C) hydrothermal technology results in the doping of carbon atom into TiO2 lattice, which makes the synthesized C-OMS@TiO2-xs are sensitive to visible light due to the changes of band gap of TiO2 nanocrystals in these samples. Notably, this phenomenon can not be found in other ordered mesoporous TiO2 based nanocomposited materials.2,21 The usage of hydrothermal technology induced modification of TiO2 materials with heteroatom in order to adjust their band gap have not been reported previously. Combination of the characteristics of large BET surface areas, ordered and uniform mesopores and visible light adsorption property, C-OMS@TiO2-xs show excellent activities and good reusability for degradation of organic pollutants such as rhodamine B (RhB), methyl orange (MO) and p-nitrophenol (PNP) irradiated with visible light.
Fig. 1 Small-angle XRD pattern of (a) as synthesized F127–C-OMS@TiO2-4.0, (b) F127–C-OMS@TiO2-4.0 and (c) P123–C-OMS@TiO2-4.0. |
Fig. 2 shows wide angle XRD patterns of various C-OMS@TiO2-xs and F127–TiO2 synthesized under the same conditions. Notably, as synthesized C-OMS@TiO2-xs exhibit several weak peaks indexed as 101, 004, 200, 105, 211 and 204 reflections, which are assigned to typical anatase phase characteristics. After calcination to remove templates, the characteristic peaks associated with anatase phase become more resolved.4,9,42 Similar result could also be observed in F127–C–TiO2, which suggests the highly crystalline degree of TiO2 active species in both C-OMS@TiO2-xs and F127–C–TiO2. Except for anatase phase, the weak peaks at around 2θ = 27.4, 55.1 and 70.2° associated with rutile phase could also be observed in C-OMS@TiO2-xs and F127–C–TiO2,4,9,42 which exists in the calcinated samples, suggesting polymorphism phenomenon of crystalline TiO2 in these samples.
Fig. 3 shows the N2 adsorption–desorption isotherms at −196 °C and Barrett–Joyner–Halenda (BJH) pore size distributions of synthesized C-OMS@TiO2-xs. The C-OMS@TiO2-xs show typical type-IV isotherms with low N2 uptake at low relative pressure, and high N2 uptake at high relative pressure, suggesting presence abundant mesopores in these samples. The N2 isotherms of C-OMS@TiO2-xs display steep increase at the relative pressure of 0.75–0.99, indicating relatively narrow pore size distributions centered at 11.1–54.2 nm. The calculated textural properties of synthesized C-OMS@TiO2-xs are summarized in Table 1. The BET surface areas and total pore volumes of C-OMS@TiO2-xs are in the range of 224–553 m2 g−1 and 0.45–1.40 cm3 g−1, respectively. It is found that the pore sizes of C-OMS@TiO2-xs increase as the TiO2 amount increases (Fig. 3b), which exhibits linear relationship (Fig. S1†). This phenomenon can be explained by an enlargement of TiO2 nanocrystals onto the network of C-OMS@TiO2-xs, which results in the larger aggregated mesopores in these samples.
Run | Samples | SBETa (m2 g−1) | Vta (cm3 g−1) | Dpb (nm) |
---|---|---|---|---|
a BET surface areas and pore volumes were estimated from N2 adsorption isotherms.b Pore size distribution was estimated from BJH model. | ||||
1 | F127–C-OMS@TiO2-2.0 | 230 | 1.28 | 54.2 |
2 | F127–C-OMS@TiO2-4.0 | 260 | 1.12 | 34.5 |
3 | F127–C-OMS@TiO2-6.0 | 303 | 1.19 | 29.1 |
4 | F127–C-OMS@TiO2-8.0 | 288 | 0.73 | 15.2 |
5 | F127–C-OMS@TiO2-9.0 | 553 | 1.40 | 8.6 |
6 | P123–C-OMS@TiO2-2.0 | 279 | 1.06 | 18.9 |
7 | P123–C-OMS@TiO2-4.0 | 224 | 0.45 | 11.1 |
Fig. 4 shows TEM and HR-TEM images of P123–C-OMS@TiO2-4.0 and F127–C-OMS@TiO2-4.0. P123–C-OMS@TiO2-4.0 shows highly ordered mesopores with hexagonal symmetry (Fig. 4a and b), and TiO2 nanocrystals species with uniform sizes were homogeneously dispersed onto the network of P123–C-OMS@TiO2-4.0 (Fig. 4b), which formed the ‘brick-and-mortar’ nanostructures. This is in agreement with small angle XRD results. Similarly, highly ordered mesopores with body centered structure (Imm) could also be found in F127–C-OMS@TiO2-4.0 (Fig. 4d). The high resolution TEM images show that the TiO2 species confined into nanopores of F127–C-OMS@TiO2-4.0 and P123–C-OMS@TiO2-4.0, exhibit several crystal lattice (Fig. 4c, e and f), which is in consistent with the wide angle XRD results. Furthermore, abundant mesopores of F127–C-OMS@TiO2-4.0 could also be confirmed by STEM image (Fig. 5a), which exhibits the signals of Ti, Si, C and O (Fig. 5b). In addition, the elemental maps indicate the signals of Ti, Si, C and O formed a “brick-and-mortar” nanostructure, which were homogeneously dispersed into F127–C-OMS@TiO2-4.0 (Fig. 5c–f).
Fig. 6 shows XPS spectra of F127–C-OMS@TiO2-4.0 and as synthesized F127–C-OMS@TiO2-4.0, which exhibit the signals of C 1s, O 1s, Ti 2p and Si 2p. The peaks associated with Ti 2p are centered at around 458.5 and 464.3 eV, which are assigned to Ti4+ in TiO2 lattices. The peak associated with Si 2p is centered at around 103.8 eV, which is assigned to Si4+ in SiO2 species. The peaks associated with O 1s are centered at around 530.0 and 533.3 eV, which are assigned to the signals of Ti–O and Si–O, respectively.44 The peaks associated with C 1s can be fitted and deconvoluted into two peaks centered at around 284.8 and 286.7 eV, which are attributed to the signals of C–C and C–O bonds respectively. The formation of C–O bond should be attributed to the doping of C atom in the lattice of TiO2 under unique high temperature hydrothermal condition, which changes the band gap of TiO2 species in C-OMS@TiO2-xs. In addition, the C content of F127–C-OMS@TiO2-4.0 was also analyzed by elemental analysis, which shows C content of 0.8 wt%, further confirming the doping of C atom in OMS@TiO2-xs. The above results confirm the successful preparation of carbon doped C-OMS@TiO2-xs nanocomposited photocatalysts, in good agreement with EDX and elemental maps results.
Fig. 6 XPS spectra of (a) as synthesized F127–C-OMS@TiO2-4.0 and (b) calcinated F127–C-OMS@TiO2-4.0. |
Fig. 7 shows UV-vis diffuse reflectance spectra of as synthesized F127–C-OMS@TiO2-4.0-as, F127–C-OMS@TiO2-4.0, P123–C-OMS@TiO2-4.0, F127–C–TiO2, F127-OMS and commercial P25. Notably, F127-OMS and commercial P25 show the adsorption edges start from 400 nm and nearly no adsorption intensity in the visible-light region. In contrast, as synthesized F127–C-OMS@TiO2-4.0, F127–C-OMS@TiO2-4.0, P123–C-OMS@TiO2-4.0 and F127–C–TiO2 show relatively weak adsorption steps in visible-light region and strong adsorption peaks in UV-light region, which start from 650 nm. The visible light response property should be attributed to their unique high temperature hydrothermal synthesis technology, which results in the doping of carbon heteroatom in the TiO2 lattices. The adjusting of band gap of TiO2 nanocrystals in porous polymers via facile high temperature solvothermal technology has been reported by us previously.37 Visible-light adsorption property of C-OMS@TiO2-xs and F127–C–TiO2 plays the key factor for their photocatalytic applications irradiated with visible light.
Fig. 8 shows photocurrent–time (I–t) curves of as synthesized P123–C-OMS@TiO2-2.0-as, as synthesized F127–C-OMS@TiO2-2.0-as, and calcinated F127–C-OMS@TiO2-2.0 under visible light irradiation (λ > 400 nm). It is well known that photoelectron chemistry test was thought to be a powerful tool to monitor the light response, generation and transportation of eCB− of various photocatalysts. In this work, the photoelectrochemical properties of C-OMS@TiO2-xs materials are studied by using the P123–C-OMS@TiO2-2.0-as, F127–C-OMS@TiO2-2.0-as and F127–C-OMS@TiO2-2.0 as the working electrode, where Pt wire and Ag/AgCl (saturated KCl) are used as the counter and reference electrodes, respectively. Under the irradiation with visible light, the photocurrent is produced and recorded. Notably, the photocurrent with different densities formed by employing the synthesized C-OMS@TiO2-xs as the working electrodes, which confirm their visible photoresponse, in agreement with the result of UV-vis diffuse reflectance spectra. Meanwhile, the generated photocurrents are reproducible and stable during five on-off intermittent irradiation cycles, which show photocurrent intensities ranged from 1.68–1.83 μA. The presence of photocurrent is mainly resulted from the fast separation and transportation of the photogenerated eCB− on the surface of the working electrodes. The higher visible photocurrent intensity indicates the higher density of photogenerated carriers, which results in the slower eCB−–hVB+ recombination rate. Compared with F127–C-OMS@TiO2-2.0, relatively higher visible photocurrent intensity of F127–C-OMS@TiO2-2.0-as should be attributed to its higher content of doped carbon.45 The above characteristics were favorable for the enhancement of their visible light induced photocatalytic activities.
Fig. 9 shows TG curves of F127–C-OMS@TiO2-4.0 and P123–C-OMS@TiO2-4.0 before and after calcination. The as synthesized samples show two weight loss steps ranged from 50 to 150 and 230 to 500 °C, which were assigned to the desorption of water and decomposition of copolymer templates in the samples. After removing the templates by calcination, the samples show only one weight loss steps ranged from 50 to 150 °C due to the desorption of water. Notably, these samples show nearly no obvious weight loss or exothermic signals in the temperatures range from 600–1000 °C, which indicates their ultrastable frameworks.
Fig. 10 shows the concentrations versus reaction time for degradation of RhB over C-OMS@TiO2-xs, F127–C–TiO2 and commercial P25 irradiated with visible light. Before irradiation, the reaction mixture was stirred in darkness for 30 min to reach adsorption equilibrium, and all the samples show limited adsorption capacities for RhB. When the reaction mixture was exposed to visible light, the concentrations of RhB quickly decreased catalyzed by C-OMS@TiO2-xs and F127–C–TiO2, which is much better than that of commercial P25. For instance, the concentrations of RhB decrease from 97.4 to 74.2 ppm only after 10 min reaction in presence of F127–C–TiO2. Further prolong the reaction time up to 30 min, the concentration of RhB was decreased up to 9.7 ppm, which can be fully decomposed after 40 min irradiation. Similarly, the concentrations of RhB change from 86.5–98.5 to 61.7–78.3 ppm after 10 min reaction in presence of C-OMS@TiO2-xs catalysts; further prolong the reaction time to 50 min, nearly all of RhB has been catalyzed decomposition. In contrast, the concentration of RhB was as high as 92.1 ppm after 30 min reaction catalyzed by commercial P25. Even prolong the reaction time to 80 min, the concentration of RhB was still up to 81.5 ppm catalyzed by commercial P25. The excellent activities of C-OMS@TiO2-xs and F127–C–TiO2 in visible light region were attributed to their enhanced visible light adsorption properties. In fact, SiO2 and TiO2 act as the role of mortar and brick in C-OMS@TiO2-xs, which formed unique “brick-and-mortar” nanostructure. The “brick-and-mortar” structure was favorable for formation of ordered mesopores in C-OMS@TiO2-xs, which strongly enhance mass transfer and exposure degree of TiO2 active sites in process of photocatalysis. Therefore, although F127–C-OMS@TiO2-2.0-as show much lower TiO2 active site in comparison with F127–C–TiO2, the degradation activity of F127–C-OMS@TiO2-2.0-as is still as comparable as that of F127–C–TiO2.
Fig. 10 Adsorption property and photocatalytic activity of various samples towards the degradation of RhB irradiated with visible light (400 < λ < 680 nm). |
The degradation processes of RhB were also monitored by UV-vis adsorption spectra (Fig. S2†). The adsorption peaks associated with RhB decreases with increase in reaction time catalyzed by F127–C-OMS@TiO2-4.0 photocatalyst. The peaks associated with RhB nearly disappeared when the reaction mixture was irradiated with visible light for 80 min, and no other additional peaks could be observed, which further confirm completely decomposition of RhB in the water. Meanwhile, the TOC values of reaction mixture catalyzed by F127–C-OMS@TiO2-4.0 and F127–C–TiO2 were also investigated (as shown in Fig. S3†), which decrease with the reaction time increase. When the irradiation time was up to 150 min, nearly 90% of organic carbon was removed from the reaction mixture irradiated with visible light, which basically avoids the secondary pollution of the water. On the other hand, C-OMS@TiO2-xs show very good reusability. For instance, the decreasing of activity of P123–C-OMS@TiO2-2.0 can not be observed after 5 cycles, suggesting the long-term stabilities of C-OMS@TiO2-xs in visible light induced photocatalysis (Fig. 11). Good reusability should be attributed to their very stable framework, abundant and ordered mesopores, which strongly enhance their anti-choking and anti-sintering abilities.
Fig. 11 Cycling of P123–C-OMS@TiO2-2.0 in degradation of RhB in the water irradiated with visible light (λ > 400 nm). |
Except for RhB, C-OMS@TiO2-xs were also very active for catalyzing degradation of MO and PNP in the water. Fig. 12 shows kinetic curves for degradation of MO over various samples irradiated with visible light. Notably, all the samples show limited adsorption contents for MO under darkness. When the reaction mixture was exposed to visible light, the concentrations of MO quickly decreased catalyzed by as made F127–C-OMS@TiO2-2.0, as made P123–C-OMS@TiO2-2.0 and F127–TiO2, nearly all of MO was decomposed (from 29.3 to 0.3 ppm) within 180 min of irradiation. In contrast, the concentration of MO was still up to 26.3 ppm after 180 min of reaction in presence of commercial P25. Similar results could also be observed for degradation of PNP, after 140 min irradiation with visible light, nearly all of PNP in the water has been catalyzed decomposition in presence of F127–C-OMS@TiO2-2.0 and P123–C-OMS@TiO2-2.0 photocatalysts (Fig. 13). The above results confirmed that C-OMS@TiO2-xs and F127–C–TiO2 could be used as visible light active, highly efficient and reusable photocatalysts for degradation of organic pollutants in the water.
Fig. 12 Adsorption property and photocatalytic activity of various samples towards the degradation of MO irradiated with visible light (400 < λ < 680 nm). |
Fig. 13 Adsorption property and photocatalytic activity of various samples towards the degradation of PNP irradiated with visible light (400 < λ < 680 nm). |
Visible light induced (λ > 400 nm) photocatalytic degradation of MO and PNP was also carried out in a cylindrical glass under irradiation by a PLS-SXE300 300 W xenon lamp equipped with a 400 nm cutoff filter. Typically, 5 mg of catalyst was added into a cylindrical glass containing 10 mL of MO (30 ppm) or 10 mL of PNP (10 ppm), which was equipped with a circulation water system to maintain a constant temperature. Before irradiation, the mixture was stirred under darkness for 30 min to achieve the adsorption equilibrium. At a given time interval of irradiation, small aliquots (0.5 mL) were withdrawn and analyzed by UV spectroscopy with the wavelength of 463 (MO) and 317 nm (PNP), respectively.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c7ra01368j |