Lei Gaoac,
Handong Li*a,
Wuyang Renb,
Gaoyun Wanga,
Hui Lia,
Zhihua Zhoua,
Haining Jia,
Xiaobin Niua and
Zhiming Wangb
aState Key Laboratory of Electronic Thin Films and Integrated Devices, School of Microelectronics and Solid-State Electronics, University of Electronic Science and Technology of China, Chengdu 610054, China. E-mail: hdli@uestc.edu.cn
bInstitute of Fundamental and Frontier Sciences, University of Electronic Science and Technology of China, Chengdu 610054, China
cMicrosystem and Terahertz Research Center, Chinese Academy of Engineering Physics, Chengdu 610200, China
First published on 23rd June 2017
Acidic potassium dichromate solutions (K2Cr2O7–H2SO4 and K2Cr2O7–HCl) are applied for patterning single crystalline Bi2Se3 thin films on Si(111) substrates. In solutions with appropriate component proportions, vertical walls and mesa-shaped structures on the etching profiles of (001) Bi2Se3 films can be achieved. Stoichiometric etching behavior is noted for Bi2Se3 in K2Cr2O7–H2SO4 etchant, while incongruently dissolution of Bi2Se3 in K2Cr2O7–HCl is observed which leaves a Se deficient layer on the etched film surface. The chemical reaction kinetics of Bi2Se3 in the two different etchants are also discussed.
However, as a key step towards device realization, patterning Bi2Se3 thin films is still of challenge. Physical bombardment of argon ions and reactive ion etching offer very little selectivity of the sample material over photoresist and carbonization of photoresist masks due to long term exposure to high energy ion beams may ensue. The complicated operation also hinders the popularity of dry-etch in processing weakly-bonded Bi2Se3. As compared to dry etching approaches, wet etching is an effective alternative due to its high etching rate, low cost and high selectivity. The etchants with different etching velocity, surface roughness, and some other characteristics can further be worked out for various purpose. Among etchants ever employed for Bi2Se3 and other chalcogenides, iodine and/or bromine based chemistries promise selective surface etching at limited rate.15 For fast chemical cutting of bismuth chalcogenides, the most popular wet etchant ever used is aqueous solutions of HNO3 and HCl mixture (diluted aqua regia).16–21 However, these highly corrosive solutions could cause a vigorous uncontrollable reaction with Bi2Se3, resulting in severe edge undercutting. The diluted aqua regia etchants become even detrimental for handling thin films because they either cause pattern disappearance or trigger the delamination of weakly adhering Bi2Se3 films from bottom substrates.22
In this work, oxidizing etchants based on K2Cr2O7–H2SO4 and K2Cr2O7–HCl solutions are used for patterning Bi2Se3 thin film electrodes on Si, respectively. K2Cr2O7–H2SO4–HCl ternary system has been verified suitable for using in etching solutions of covalent GaAs and InP wafers before.23 It's demonstrated that the simpler K2Cr2O7–H2SO4 and K2Cr2O7–HCl binary aqueous solutions can also produce mesa-shaped structures with vertical walls of layered Bi2Se3 thin films in this research. Superior surface morphologies of the etched Bi2Se3 (001) over the un-etched ones are obtained in solutions with proper acidities. However, incongruently etching behaviors on the Bi2Se3 surfaces are noted that a Se depletion surface layer is formed on Bi2Se3 etched in the K2Cr2O7–HCl solutions.
The K2Cr2O7–HCl (H2SO4) etchants are prepared by intermixing 9 v/v% K2Cr2O7 and 48 v/v% HCl (98 v/v% H2SO4) solutions in volume proportions of 1:1, 1:2, and 1:3 (thereafter denoted by 1:n K2Cr2O7–HCl (H2SO4), n = 1, 2, 3), respectively at room temperature. As in Table 1, the acquired acidities, as represent by H+ concentration ([H+]) in the solutions, are calculated to be 6 mol L−1, 8 mol L−1, and 9 mol L−1 for the 1:1, 1:2, and 1:3 K2Cr2O7–HCl etchants, respectively. For the 1:1 to 1:3 K2Cr2O7–H2SO4 etchants, [H+] values are 9 mol L−1, 12 mol L−1, and 13.5 mol L−1, respectively. The Bi2Se3 films are etched in these aqueous acidic solutions for given time and no stirring is carried out to isolate the influence from hydromechanical effect. After etching, the samples are rinsed in acetone until the photoresist can be stripped. To investigate the dissolution of Bi2Se3, ascertain the character of corresponding reactions and determine limiting stages of the process, various methods are involved in the experiments. The thickness of the etched films is measured by a surface profilometer (Dektak150, Veeco). Optical microscopy (Olympus BX51), atomic force microscopy (AFM), and scanning electron microscopy (SEM) are employed to investigate the surface morphologies of the obtained patterns. Surface structural and compositional details of etched samples are further studied by Raman and electron dispersive spectroscopy (EDX), respectively. The chemical identification and binding energy study of the etched Bi2Se3 films are conducted by X-Ray Photoelectron Spectroscopy (XPS, Omicron).
Etch solution | Proportion | [H+] (mol L−1) |
---|---|---|
K2Cr2O7–HCl | 1:1 | 6 |
K2Cr2O7–HCl | 1:2 | 8 |
K2Cr2O7–HCl | 1:3 | 9 |
K2Cr2O7–H2SO4 | 1:1 | 9 |
K2Cr2O7–H2SO4 | 1:2 | 12 |
K2Cr2O7–H2SO4 | 1:3 | 13.5 |
For better describing the dissolving properties of Bi2Se3 in acid K2Cr2O7 solutions, the etching depths (θ) of the Bi2Se3 film are measured at different time intervals (t). A typical θ–t curve of Bi2Se3 in 1:2 K2Cr2O7–HCl etchant is shown in Fig. 2(a), and a constant etching rate of ∼120 nm min−1 is calculated from its linear fitting, indicating a rate-controlled etching reaction. It must be pointed out that the etching almost ceases at depth of 350 nm which is possibly due to the consumption of [H+] in the solution. Also noted from the θ–t curve is the reaction delay of Bi2Se3 during the initial 15 seconds before the balanced etching rate can be reached. Such behavior is also observed in all other reactions. By carefully excluding any extrinsic contamination on sample surfaces, we suppose the initial dissolving of Bi2Se3 is hindered by a thick native oxidized layer formed on each sample surface which has suffered long-time exposure in air. The induction period varies a lot for different Bi2Se3 samples, despite of the same acidity and temperature conditions are adopted in those reactions, which is ascribed to the reaction dependence on different chemical compositions and/or thicknesses of the oxidized layers on Bi2Se3 samples, and would not be discussed here. After the induction period, the reaction accelerates and the dissolving process of Bi2Se3 exhibits clear dependence on both the reaction temperatures and acidities of the etchants. Fig. 2(b) shows the quantitative Bi2Se3 etching rate dependence on acidities of K2Cr2O7–HCl and temperatures (20 °C to 45 °C). In the [H+]: 6 mol L−1 etchant, the chemical reaction is weak that rather slight dissolution of the film can be detected even after the solution temperature is elevated from 20 °C to 45 °C (actually, the etching rate is only increased from 10 nm min−1 to a few tens of nanometers per minute as temperature ramps up from 20 °C to 45 °C). While after the [H+] of the K2Cr2O7 etchants is increased larger than 8 mol L−1, the chemical reaction is obviously activated and the etching rates yield rapid increase at elevated temperatures. As judged from the measured rate curves depicted in Fig. 2(b), the dissolution of Bi2Se3 in 1:3 K2Cr2O7–HCl is nearly three times faster than it in 1:2 K2Cr2O7–HCl etchant at room temperature. To quantitatively describe the chemical reaction intensity of Bi2Se3 in the oxidizing acids with different [H+], we calculate the activation energies of etching reactions of Bi2Se3 in 1:1, 1:2, and 1:3 K2Cr2O7–HCl solutions (the corresponding [H+] is 6 mol L−1, 8 mol L−1, and 9 mol L−1, respectively) from the plots using Arrhenius equation for these curves shown in Fig. 2(b), and the calculated activation energies are 0.88 eV, 0.74 eV, and 0.47 eV, respectively. It thus strongly manifests that the chemical reaction barrier of Bi2Se3 in the oxidizing acids decreases dramatically as the acidity increases in the etching solutions. However, such an intense reaction leads to severely uneven etching of the patterned film. As shown in inset of Fig. 2(b) is an optical microscopic picture of slightly etched Bi2Se3 by 1:3 K2Cr2O7–HCl solution at room temperature, on which it can be clearly figured out that the areas near the grid corners are attacked much faster than the other regions. As the etching proceeds, undesired “W”-shape depth profiles of the film gradually evolve and part of the Bi2Se3 grid pattern gets eventually dissolved.
Almost the same etching behaviors of Bi2Se3 in K2Cr2O7–H2SO4 etchants are observed. The 1:2 in K2Cr2O7–H2SO4 ([H+]: 12 mol L−1) etchant also yields the same etching rate of ∼120 nm min−1 as obtained in the 1:2 in K2Cr2O7–HCl and can produce “U” shape etching profiles of the Bi2Se3 films. Anyway, the electronic characteristics of electrodes and heterojunctions based on the etched Bi2Se3 subject on the microscopic surface properties, it's therefore necessary to analyze the morphologies and stoichiometry of the Bi2Se3 surfaces etched by these two kinds of etchants. As illustrated in Fig. 3(a) is a SEM image of an as-deposited Bi2Se3 thin film. High dense growth spirals surrounded by straight steps are observed in the as-grown Bi2Se3 thin films (highlighted by dashed triangles in Fig. 3(a)). As measured by AFM, the root mean square (RMS) roughness of such surface is ∼3 nm (in area of 5 × 5 μm2), as shown in Table 2. After being immersed in 1:2 K2Cr2O7–H2SO4 solution for 30 seconds which corresponds to an etching depth of ∼60 nm, these pyramid morphologies completely vanish and a surface decorated with large amounts of irregular-shaped islands sized from ∼20 nm to ∼300 nm comes out as exhibited in Fig. 3(b). The surface morphology does not improve too much (RMS roughness ∼2.5 nm) as compared to the as-deposited Bi2Se3 film. On such etched surface, a Se:Bi mole ratio of ∼1.60 is detected by EDX measurement. The Se:Bi mole ratio doesn't change significantly after a further 30 seconds etching period indicates a stoichiometric dissolution of Bi2Se3 in the 1:2 in K2Cr2O7–H2SO4 etchant. Fig. 3(c) shows a SEM image taken from a Bi2Se3 film etched in 1:2 in K2Cr2O7–HCl solution at ∼60 nm depth too. A much smoother surface (RMS roughness ∼1.5 nm) is obtained for Bi2Se3 in this etchant. Not identical to the case of Bi2Se3 in 1:2 in K2Cr2O7–H2SO4, Se:Bi mole ratio on the 1:2 in K2Cr2O7–HCl etched surface is ∼1.1 as measured by EDX, implying a Se-dissolving preferred reaction kinetics. As etching proceeds to ∼270 nm depth, only Bi signal from the film can be detected by EDX indicating a full depletion of Se. It should be noted that the good epitaxial character with two-dimensional surface terrace-step structures of initial Bi2Se3 films disappears after being etched in both solutions, which strongly implies that both etching processes would cause amorphous surface parts of the Bi2Se3 films. It's thus also reasonable to attribute the nano-sized islands with irregular shapes (as shown in Fig. 3(b) and (c)) to be amorphous Bi2Se3 deposits after etching.
Fig. 3 SEM images of an as-deposited Bi2Se3 surface (a) and Bi2Se3 surfaces etched in 1:2 K2Cr2O7–H2SO4 etchant (b) and 1:2 K2Cr2O7–HCl etchant (c), respectively. |
Sample surface | RMS roughness | Se:Bi mole ratio |
---|---|---|
Un-etched Bi2Se3 thin film | 3 nm | 1.6 |
In 1:2 K2Cr2O7–H2SO4 solution for 30 s | 2.5 nm | 1.6 |
In 1:2 K2Cr2O7–HCl solution for 30 s | 1.5 nm | 1.1 |
It's well known that wet chemical etching proceeds by oxidation of the semiconductor constituents followed by chemical dissolution of the oxides in suitable solvents. For etching covalent chalcogenides such as CdSe, CdTe, and HgCdTe, different dissolving rates between cations and chalcogens are often observed because the hydration of cations is much easier than that of nonfully-oxidized chalcogens on the material surfaces.26–29 As a result, the etched surfaces of chalcogenides are usually cation-deficient. While no cation-deficient surfaces of etched Bi2Se3 are obtained in our experiments, which suggests quite different reaction kinetics of layered Bi2Se3 as compared to that of covalent chalcogenides in oxidizing acids etchants. To further understand the chemical reaction kinetics of Bi2Se3 in oxidizing acids with different components, XPS study is carried out for characterizing the chemical status of Bi2Se3 surfaces etched in different acid K2Cr2O7 solutions.
As shown in Fig. 4 are core level spectrum of Bi and Se elements detected by XPS from the samples etched in 1:2 K2Cr2O7–HCl and 1:2 K2Cr2O7–H2SO4 etchants with etching depth of ∼60 nm, respectively. The binding energies (BE) obtained in the XPS analysis are standardized for specimen charging using C 1s peak as the reference at 284.8 eV. To precisely determine the peaks' positions, Lorentz–Gauss profiles and Shirley background have been taken for the deconvolution. As indicated in Fig. 4(a) is Bi 4f spectrum from the K2Cr2O7–H2SO4 etched Bi2Se3 sample, in which the intensity contribution for spin–orbit-splitting Bi 4f peaks (4f7/2 and 4f5/2) from either Bi–O bonding30,31 or Bi–Se bonding can be clearly distinguished upon deconvolution. The intensities of Bi–O bonding Bi peaks are much stronger than that of Bi–Se bonding Bi peaks, which suggest there exists a bismuth oxide (BiOx) thin layer deposited on the Bi2Se3 surface during etching. While for the K2Cr2O7–HCl etched Bi2Se3 case, only a pair of Bi 4f peaks located at 158.82 eV and 164.11 eV are observed which can be precisely attributed to Bi–Se bonding of pure Bi2Se3 (Fig. 4(b)).32–34 Peaks referred to Se 3p1/2 and Se 3p3/2 can also be figured out in both fitted XPS spectra as exhibited in Fig. 4(a) and (b), and the broaden peak profiles depict a mixed valence states of Se on both samples.35 The valence states of Se from Bi2Se3 films after etched by K2Cr2O7–H2SO4 and K2Cr2O7–HCl are further investigated by analyzing the peak fitted Se 3d (3d5/2 and 3d3/2) spectra as illustrated in Fig. 4(c) and (d), respectively. In either Se 3d curve, the pair of high BE component peaks belong to Se–Se bonding of element Se and the other pair are related to Bi–Se bonding, respectively. And no traces of any selenium oxides can be found on the etched Bi2Se3 surfaces in our XPS studies.30 Therefore, it's reasonable to determine that there's only a Se2− → Se0 oxidizing reaction happens for the Se element in both etching processes and the free element Se reactants are deposited onto the Bi2Se3 surfaces. Further, peak intensity contribution from Se–Se bonding dominates in Se 3d spectra of the K2Cr2O7–H2SO4 etched Bi2Se3 sample while it becomes not prominent in K2Cr2O7–HCl etched one, which manifests that there're more Se deposits residual on K2Cr2O7–H2SO4 etched Bi2Se3 surface than those on K2Cr2O7–HCl etched one.
Based on the XPS observations, it should be feasible to determine that the surface chemistry is predominated by bismuth oxides and element Se all through the etching procedure in K2Cr2O7–H2SO4 solutions. Therefore the surface reaction kinetics are only subjected by the rate of reactants reaches and leaves the etched surface.36 As to our knowledge, there's only tempered chemical reactions happen between bismuth oxides and concentrated acids (such as H2SO4 and HCl) at room temperature. So do them between element Se and concentrated sulphuric acid. As a result, congruently dissolving of Bi and Se will dominate in the etching reaction which is confirmed by our experiment observations.
On the other hand, the valence states of Bi in Bi2Se3 remains intact during etching in K2Cr2O7–HCl solutions. It's thus suggested that the etching action on the Bi2Se3 surface is fully triggered by dissolving of Se. As a result, it leads to the observed incongruently etching behaviors of Bi2Se3 in K2Cr2O7–HCl etchants.
This journal is © The Royal Society of Chemistry 2017 |