DOI:
10.1039/C7RA05386J
(Paper)
RSC Adv., 2017,
7, 37778-37786
Preparation of an ion imprinted functionalized mesoporous silica for rapid and specific absorption Cr(III) ions in effluents†
Received
12th May 2017
, Accepted 25th July 2017
First published on 1st August 2017
Abstract
We developed an effective and selective method to remove Cr(III) ions in acidic effluents. This method used combined ion imprinted technology with mesoporous silica materials. Cr(III) ion imprinted mesoporous silica (CrIMS) was synthesized and used as an excellent adsorbent. Iminodiacetic acid (IDA) was silanized, and acted as a functional monomer. The chemical groups, thermal stability, porosity and highly ordered morphology of CrIMS were characterized by Fourier transform infrared spectroscopy (FTIR), thermogravimetric analysis (TGA), Brunauer–Emmett–Teller (BET) isotherms, X-ray diffraction (XRD), transmission electron microscopy (TEM) and scanning electron microscopy (SEM). The Brunauer–Emmett–Teller (BET) surface area was 856.24 m2 g−1. The saturated adsorption capacity of CrIMS towards Cr(III) ions reached up to 63 mg g−1 at pH 4.5. At a concentration of 200 mg L−1, the adsorption of Cr(III) ions reached equilibrium within 5 min and 20 min at pH 4.5 and pH 3.0, respectively. The CrIMS showed highly specific adsorption capacity and the imprinting factor was up to 4.03 at pH 3.0. The adsorption capacity of Cr(III) ions was remarkably higher than other co-existing metal ions. After eight adsorption–regeneration cycles, the adsorption efficiency of CrIMS still reached above 94.1%. The CrIMS could effectively remove Cr(III) ions below the discharge standard of China in real sample treatment.
1. Introduction
Electroplated chromium coatings are widely used, thanks to their excellent properties. The hexavalent Cr has been applied for many years in traditional techniques. Because of the serious toxicity of Cr(VI), Cr(III) has been applied as a substitute in more environmentally friendly processes.1 Besides, chromium is widely used in many other industries, such as wood preservation, leather tanning, textiles, metallurgy, and pigments.2 Chromium is easily converted to a serious pollutant and is harmful to the environment during widespread use.3,4 Cr(III) ions usually exist in effluents from many industries and excessive emissions can also pollute the environment, although the toxicity of Cr(III) ions is much lower. On the other hand, Cr(III) can transform to Cr(VI), resulting from the effects of pH, oxidizing agent (O2) and so on.4 Thus, chromium continues to enter food chain organisms, which may lead to carcinogenic, allergenic and mutagenic effects.5,6 Therefore, it is necessary to design a safe and clean procedure for the efficient removal of Cr(III) ions from effluents.
Various methods and technologies to remove Cr(III) ions or other metal ions from effluents to an acceptable concentration level have been investigated, such as liquid–liquid extraction,7 ion-exchange,8 adsorption,9 chemical precipitation9 and electrochemical reduction.10 However, the use of organic solvent is inevitable during liquid–liquid extraction. Besides, the electrochemical reduction requires extra electrical energy. Among these methods, adsorption has been regarded as the most promising and widely used method due to its high efficiency, simplicity, economy, and environmentally friendly behavior. Activated carbons and low cost adsorbents, such as agricultural residues11 and natural products12 can also act as adsorbents. These adsorbents usually have low loading capacities and weak interactions with metallic cations.13,14 Inorganic/organic hybrid materials,15 chelating resin16 and carbon nanotubes17 have been investigated as adsorbents used in the removal of Cr(III) ions and other heavy ions from effluents. However, the designs of the above adsorption materials seldom consider the structure of the target and the characteristics of effluents, such as acidity, interfering components and initial metal concentration, and there are always some limitations in their practical applications.18 Therefore, searching for more effective adsorbents to remove heavy metal ions requires a continuous effort for many researchers.
Mesoporous materials possess the large internal surfaces, which highly enhance the capacity of catalytic, absorptivity and the speed of mass transfer. Mesoporous silica, one of typical mesoporous materials, is a kind of an inexpensive and robust porous silica-based solid. Since a new family of mesoporous molecular sieves was prepared with liquid crystal templates in 1992,19 ordered mesoporous silica has attracted much concern in different fields, due to their uniform pore sizes within the range of a few nanometers and their large surface areas. Ordered mesoporous silica complements conventional zeolites in applications, including adsorption,20 catalysis,21 drug delivery22 and sensing.23 MCM-41 and MCM-48,24 which have been synthesized at high pH by using cationic surfactants templates, are the two common series of mesoporous silica. Besides, anionic and nonionic surfactants have also attracted interest as templates for mesoporous materials. Silica precursors usually need to be hydrolyzed in low pH (SBA-15, SBA-16).25 SBA-15 possesses thicker framework walls than MCM-41, and thus exhibits a higher thermal and hydrothermal stability. Therefore, SBA-15, synthesized in strongly acidic medium, makes it a good candidate as an adsorbent support material for removal of Cr(III) ions from acidic effluents. Many researches have focused on modification of SBA-15 by some functional groups (e.g. carboxyl, amine),26 but the simple modified mesoporous silica hardly possess specific recognition ability for Cr(III) ions and high adsorption capacities in acidic medium.
With the pioneering work conducted in the 1990s, molecular imprinting technology(MIT) has increasingly developed27 and has attracted considerable attention as a new fabrication technology of bionic receptors.28 In general, molecular imprinting polymers (MIPs) are prepared by the copolymerization of functional monomers and cross-linkers in the presence of target analytes that act as template molecules, which results in selective cavities in a 3D-polymeric network and shows great affinity with target analytes.29,30 Owing to their high selectivity, inherent simplicity, reusability, physical robustness and cost-effectiveness, MIPs are widely used in different fields, such as purification and separation,31 chemo/biosensing,32 drug delivery,33 and catalysis.34 The molecular imprinting technique has also been applied to prepare ion imprinted polymers (IIPs).35 However, traditional IIPs exhibit a low adsorption capacity and poor site accessibility toward targets, as the binding sites are embedded within a highly cross-linked polymer matrix. In order to design high selective adsorbent with large surface areas, applying imprinting technology to mesoporous materials is a promising strategy, which gained considerable interest over the past few years.35,36 In those ion imprinted mesoporous silicas, the selectivity toward template metal ions was improved without considering their adsorption capacities in acidic medium. Co-condensation is one of common strategies to modified mesoporous silica materials.37 Compared to postsynthetic functionalization (grafting), co-condensation modification is the simultaneous addition of the corresponding silica and structure-directing agents (SDAs) with organosilica precursors and templates. The organo-functional groups covalently anchor in the pore walls, and it can effectively overcome some shortcomings of grafting synthesis, such as the loss of surface area, pore blocking, and heterogeneous distribution of recognition sites.38
In this work, we designed and fabricated a novel, highly ordered Cr(III) ions imprinted mesoporous silica (CrIMS) functionalized by iminodiacetic acid (IDA) for directly removing and recycling Cr(III) in a strongly acidic medium (Scheme 1). IDA and (3-glycidyloxypropyl)trimethoxysilane (GLYMO) were reacted to synthesize a precursor GLYMO–IDA, which acted as the functional monomer. Tetraethoxysilane (TEOS) was chosen as the cross-linker, while P123 was used as the SDAs. The synthetic CrIMS was characterized by small angle X-ray diffraction (XRD), transmission electron microscopy (TEM) and nitrogen adsorption–desorption measurement. Its adsorption behavior in aqueous solutions was investigated and compared with non-imprinted mesoporous silica (NIMS). Eventually, the ability of CrIMS to remove Cr(III) efficiently was demonstrated in highly acidic actual effluents samples.
|
| Scheme 1 Schematic procedure for synthesis of Cr3+ imprinted mesoporous silica. [GLYMO: (3-glycidyloxypropyl) trimethoxysilane, IDA: iminodiacetic acid, P123: poly(ethylene glycol)-block-poly(-propylene glycol)-block-poly(ethylene glycol), TEOS: tetraethoxysilane, SDAs: structure-directing agents]. | |
2. Materials and methods
2.1. Materials
All reagents and solvents were of AR grade and used without further purification unless otherwise noted. Tetraethoxysilane (TEOS) was obtained from Aladdin Reagent Company (Shanghai, China), while (3-glycidyloxypropyl)trimethoxysilane (GLYMO) was purchased from J&K-Scientific Chemical Reagent Company (Beijing, China). Poly(ethylene glycol)-block-poly(-propylene glycol)-block-poly(ethylene glycol) (P123, EO20PO70-EO20) was received from Sigma-Aldrich (Shanghai, China). Iminodiacetic acid (IDA) was obtained from Alfa Aesar (Shanghai, China). Hexamethylene tetraamine, nitric acid, CrCl3·6H2O, ZnCl2·6H2O, CdCl2·2.5H2O, Cu(NO3)2·3H2O, Pb(NO3)2, MnCl2·4H2O and FeCl3·6H2O, were provided by Tianjin Chemical Reagent Company (Tianjin, China). Doubly distilled water (DDW) was used for all dilutions except for the real sample.
2.2. Preparation of GLYMO–IDA silane
GLYMO–IDA silane was prepared basing on a published method with some modifications.18 IDA (30 mmol) and 50 mL of DDW were mixed in a 100 mL single-necked flask. The pH of the solution was then adjusted to 11 with 10 mol L−1 NaOH. Then, the flask was cooled by using ice-bath and 6 mmol of GLYMO was slowly mixed in the solution. The mixture was heated in water-bath at 65 °C for 6 h with stirring, followed by cooling the resultant in an ice-bath for 10 min. When the temperature of the resultant dropped to 0 °C, 6 mmol of GLYMO was further added slowly with vigorous stirring. The mixture was heated in water-bath at 65 °C for 6 h with stirring, again. Similarly, 7 mmol of GLYMO was again added into the above mixture and incubated overnight with stirring at 65 °C. Finally, the pH of the GLYMO–IDA-silane solution was adjusted to 6 by using concentrated HNO3. This synthesized compound solution was stored in a refrigerator at 4 °C.
2.3. Preparation of CrIMS and NIMS
CrCl3 (1 mmol) and GLYMO–IDA (2 mmol) were mixed in 10 mL of DDW and stirred at 40 °C for 2 h to form a pre-assembly solution. Meanwhile, 2.0 g of P123 and 10 mL of 12 mol L−1 hydrochloric acid were mixed in 50 mL of DDW and kept stirring for 2 h at 40 °C. The pre-assembly solution was dropped into this solution. The mixed solution was kept stirring for 1 h. Then, TEOS (15 mmol) was dropped into the mixture and the mixture was kept stirring for 12 h. The resultant solution was transferred into a hydrothermal reactor and reacted at 85 °C for 48 h. The collected products were eluted by using Soxhlet extraction with an ethanol–hydrochloric acid solution (9:1, v/v) to remove the Cr(III) ions and the surfactant. After that, the final CrIMS was acquired and dried in a drying cabinet. The non-imprinted mesoporous silica (NIMS) was synthesized in parallel but without the addition of the Cr(III) ions.
2.4. Apparatus and analytical conditions
Small angle X-ray diffraction (XRD) measurements were conducted with a Bruker D8 Advance Scattering system using Cu Kα (λ = 1.5405 Å) radiation over a range of 0.5–5° 2θ. Fourier transform infrared spectra (FTIR) were recorded using a Varian DRX-400 Fourier Transform Spectrophotometer. Transmission electron microscopy (TEM) analysis was performed by using a JEM-2010HR at 120 kV (JEOL, Japan). Scanning electron microscopy (SEM) images were taken on a ZEISS Ultra 55 microscope. N2 adsorption–desorption measurements were carried out using a surface area and pore size analyzer from Beishide Instrument (Beijing). Surface areas were calculated by the Brunauer–Emmett–Teller (BET) method, and the pore volume and pore size distribution were calculated using the Barrett–Joyner–Halenda (BJH) model. Solid-state 13C and 29Si NMR were carried on a Bruker Ascend III 400 HD. Thermogravimetric analysis (TGA) curves were obtained by heating the sample from 30 to 700 °C at a heating rate of 10 °C min−1 under an air atmosphere using a thermogravimetric analyzer (NETZSCH, Germany). Metal ion concentrations were recorded on a Varian 730 ES Inductively Coupled Plasma Emission Spectrometer.
2.5. Adsorption experiment
Adsorption experiments were investigated by using 10 mg CrIMS or NIMS and 10 mL solution at 25 °C. The pH of the solution was adjusted by using nitric acid–hexamethylenetetramine buffer solution. In the pH test, CrIMS or NIMS were added at a different pH (2.0–6.0) of Cr(III) ions solution (200 mg L−1) in each vial. The calculated imprinting factor (IF) was defined as IF = Bi/Bn, where Bi and Bn represented the binding capacity of CrIMS and NIMS, respectively. After each adsorption cycle, the CrIMS or NIMS were separated by centrifugation, and the residual concentration of Cr(III) ions in the supernatant was measured. All the adsorption experiments were conducted in triplicate, and the mean values are reported.
The isothermal adsorption experiments were carried out by using a series of Cr(III) ions solution in the range of 1 to 400 mg L−1. The adsorption kinetics tests were performed using Cr(III) ions solutions of two different concentrations (20 and 200 mg L−1). After shaking for regular time, the CrIMS was separated, and the residual concentration of Cr(III) ions in the solution was measured by ICP-MS.
In order to measure selectivity of the CrIMS, the mixed solutions containing Cr3+, Zn2+, Cd2+, Cu2+, Pb2+, Mn2+ and Fe3+ (1 mmol L−1) were used, and the pH of each solution was maintained at 4.5.
2.6. Reusability and reproducibility
Cr(III) ions solution of concentration 200 mg L−1 at pH 4.5 was used for testing the reusability and reproducibility of the CrIMS. In each cycle, the Cr(III) ions absorbed by the CrIMS was eluted with 4 mL of 2 mol L−1 HCl. The CrIMS was washed thrice with DDW, neutralized with 1 mol L−1 NaOH, again rinsed thrice with DDW, and dried. The dried CrIMS was then used for the next adsorption cycle. The same CrIMS was reused 8 times for adsorption of Cr(III) ions to measure its reusability. Additionally, five batches of CrIMS prepared at different times and were employed to evaluate the reproducibility of CrIMS.
2.7. Removal of Cr(III) ions from water sample
The sample of electroplating effluent was collected in a polyethylene bottle from Dawang Electroplating Industrial Park (Guangdong, China) with pH 3.0 and Cr(III) ions concentration of 26 mg L−1. The water sample was filtered through a 0.45 μm micro filtration membrane to remove all impurities. Then, the CrIMS was used to adsorb Cr(III) ions from 10 L of the effluent. The residual concentration of Cr(III) ions in the solution was analyzed by ICP-MS. The recycle method of the CrIMS was same as that of the reusability experiment mentioned above.
3. Results and discussion
3.1. Characterization of CrIMS
3.1.1. FT-IR spectra. The FT-IR spectra of the samples are displayed in Fig. 1. The wide and strong absorption band at 3300 cm−1 was ascribed to the stretching vibration of O–H and the absorption band at 1626 cm−1 was attributed to the bending mode of O–H in SBA-15, NIMS and CrIMS.18,39 The characteristic peaks of the Si–O–Si group and the Si–O are found at 1060 cm−1 and 795 cm−1, which proves that the matrix materials of these three samples are silica. The characteristic peaks of the CO group was found at 1731 cm−1 on the curve of NIMS and CrIMS, confirming that GLYMO–IDA was successfully embedded in the silica matrix.
|
| Fig. 1 FT-IR spectra of SBA-15, NIMS and CrIMS. | |
3.1.2. Solid-state 13C and 29Si NMR spectra. The solid-state 13C NMR spectra of NIMS and CrIMS (Fig. 2) showed the characteristic peaks (peak 1–6), which corresponded to the structure of GLYMO–IDA. The signal of carbon C-1 directly bound to the Si atom was presented at 7 ppm. The resonance peak at 21 ppm corresponded to carbon C-2 of the propyl chain in GLYMO–IDA. The peaks at 56, 64, and 72 ppm could be ascribed to C-5, C-3 and C-4, respectively. The peak for the carboxyl carbons of IDA moieties appeared clearly at 169 ppm.18
|
| Fig. 2 Solid-state 13C NMR spectrum of CrIMS and NIMS. | |
The spectra of solid-state 29Si NMR of NIMS and CrIMS (Fig. 3) presented the peaks of T3, Q2, Q3 and Q4 (−65, −93, −102 and −111 ppm, respectively). The T3 silicon signals represented the structure of (SiO)3SiR, which could be attributed to the Si of functional monomer (GLYMO–IDA). Besides, the peaks of Qn (n = 2, 3 and 4) corresponded to the structure of (SiO)nSi(OH)4−n, which were common signals of mesoporous silica.40,41
|
| Fig. 3 Solid-state 29Si NMR spectrum of CrIMS and NIMS. | |
Based on the analysis of the solid-state 13C and 29Si NMR, it could be proved that GLYMO–IDA was successfully incorporated into the mesoporous silica.
3.1.3. XPS analysis. The XPS spectrum of CrIMS is displayed in Fig. 4. The signals of C1s and N1s indicated that GLYMO–IDA has been involved in CrIMS. Besides, the signal of Cr was hardly to be detected, which revealed that the Cr(III) ions were eluted.
|
| Fig. 4 XPS spectrum of CrIMS. | |
3.1.4. XRD patterns. The small angle XRD pattern of CrIMS is shown in Fig. 5. Three characteristic diffraction peaks of (100), (110) and (200) were observed in the region 2θ = 0.5–2.0°, which revealed that the CrIMS owned a highly ordered 2D meso-structure with typical hexagonal P6mm symmetry. Besides, the small angle XRD patterns of CrIMS and NIMS both consistented with the pattern of SBA-15.
|
| Fig. 5 The low-angle XRD pattern of SBA-15, NIMS and CrIMS. | |
3.1.5. Morphological characteristics. The SEM image (Fig. 6) of CrIMS displayed a regular morphology and were in the shape of short pillars. The TEM image (Fig. 6) revealed that CrIMS persevered ordered porous structure and well-formed hexagonal pore arrays. The average pore diameter was about 6.25 nm and the average wall thickness is about 3.2 nm. The SEM and TEM images of CrIMS and NIMS (Fig. S1 and S2†) displayed no significant difference in the highly ordered mesoporous structure (SBA-15) (Fig. S3 and S4†).
|
| Fig. 6 SEM and TEM image of CrIMS. | |
3.1.6. BET analysis. The porous structure of the CrIMS is one of significant factors for the adsorption of Cr(III) ions. The experiment of N2 adsorption–desorption was carried out to investigate the porosity of CrIMS. A type IV isotherm with a hysteresis loop is displayed in Fig. 7, which confirms mesoporous characteristics. The insert picture in Fig. 7 presented the mean pore size, which was estimated by the Barrett–Joyner–Halenda (BJH) method to be 6.55 nm, which was consistent with the TEM image. The Brunauer–Emmett–Teller (BET) surface area was 856.24 m2 g−1 while the pore volume was 1.45 cm3 g−1. All of these results confirmed that the resultant CrIMS possessed a typical SBA-15 mesoporous structure.
|
| Fig. 7 N2 adsorption–desorption isotherm. | |
3.1.7. TGA analysis. The curves of SBA-15 and CrIMS in TGA analysis were displayed in Fig. 8. The weight loss of SBA-15 and CrIMS occurred from room temperature to 130 °C, which was attributed to the release of adsorbed water. The second weight loss of SBA-15 (5.35%) resulted from the loss of the hydroxyl groups.42 CrIMS had more obvious second weight loss (24.67%), which was mainly caused by the loss of the organic groups from GLYMO–IDA. Based on the weight loss in the TGA analysis, it was indicated that the organic groups from GLYMO–IDA were successfully combined with the silica matrix.
|
| Fig. 8 TGA curves of SBA-15 and CrIMS. | |
3.2. Binding study
The complexation between Cr(III) ions and IDA groups is distinctly influenced at different pHs. The effects of solution acidity on the adsorbed capacity and the imprinting factor (IF) of CrIMS were investigated. Since Cr(III) ions may convert to Cr(OH)3 at a high pH, the experiment was carried out from pH 2.0 to pH 6.0, shown in Fig. 9. The binding capacity of CrIMS toward Cr(III) ions was positively correlated with the pH, while the IF showed a negative one. The largest adsorption capacity (approximately 71 mg g−1) and IF (4.65) was observed at solution pH of 6.0 and 2.0, respectively. The decrease of binding capacity at lower pH could be attributed to the protonation of the donating nitrogen atoms and the lower dissociation extent of the carboxyl groups in the imprinting cavities, reducing the extent of complexation between the Cr(III) ions and the IDA groups. CrIMS possessed imprinting cavities and could specifically adsorb the templates, which was a stronger force compared with the nonspecific adsorption of NIMS. Thus, the IF values tended to be smaller at higher pHs.
|
| Fig. 9 The effect of pH on adsorption capacity and IF of CrIMS (experimental conditions: used 10 mL of 200 mg L−1 Cr(III) ion solution, solid weight 10 mg, T = 298 K). | |
In this work, we intended to construct a novel Cr(III) ions imprinting mesoporous silica material to remove Cr(III) ions from effluent at low pH. Moreover, when the pH value was below 4.5, the binding capacity was low. Besides, the initial pH of the real sample we chose is 3.0. Therefore, we chose pH 4.5 and pH 3.0 for conducting following adsorption tests.
The results of isothermal adsorption experiments were presented in Fig. 10. The binding capacities of Cr(III) ions on the CrIMS and NIMS were nonlinear and increased with the increase of the initial concentration of Cr(III) ions. The CrIMS reached a saturated adsorption value (approximately 63 mg g−1) when the initial concentration of Cr(III) ions was 200 mg L−1 at pH 4.5. At pH 3.0, the binding capacity still reached 51 mg g−1. The two saturated adsorption values were both higher than that of NIMS. These results proved that the effect of imprinting combined with the chelate action enhanced the affinities with Cr(III) ions and binding capacities of CrIMS which owns specifically binding sites.
|
| Fig. 10 Adsorption capacity of CrIMS and NIMS(Experimental conditions: used 10 mL of different concentrations of Cr(III) ion solution, solid weight 10 mg, T = 298 K). | |
3.3. Kinetic study
The kinetic study was undertaken at two different concentrations (20 and 200 mg L−1) of Cr(III) ions. As the results were shown in Fig. 11, at the same pH, equilibrium adsorption time is longer when the initial concentration of Cr(III) ions is higher. For the Cr(III) ions concentration of 20, 200 mg L−1, the time to reach equilibrium was 3 min and 5 min at pH 4.5 respectively, which was much shorter than that of typical MIPs,43 and it corresponded with common imprinted mesoporous silica.37,44 The short equilibrium adsorption time resulted from the nanometer-sized wall thicknesses and narrow pore size distribution of the mesoporous silica, which significantly enhanced the specific surface area and accelerated mass diffusion and transportation of adsorption processes.35 Therefore, the Cr(III) ions were more accessible to the binding sites of imprinted mesoporous silica. We also found the pH could affect the equilibrium adsorption time. For the Cr(III) ions concentration of 20 and 200 mg L−1, the time to reach equilibrium was 10 min and 20 min at pH 3.0, respectively.
|
| Fig. 11 Adsorption kinetics of CrIMS (used 10 mL solution, 10 mg adsorbent, T = 298 K). | |
3.4. Selectivity study
In order to investigate the ability of selectively recognition of CrIMS, we chose Zn2+, Cd2+, Cu2+, Pb2+, Mn2+ and Fe3+ to performed competitive adsorption tests. These ions could coexist in effluents with Cr(III) ions, and they have similar ionic radius with Cr(III) ions. In addition, Fe3+ has the same charge with Cr3+ and is often detected at high concentrations in some water samples. As shown in Fig. 12, the adsorption capacities of NIMS toward all the ions were not significantly different, while that of CrIMS to Cr(III) ion was much higher than its adsorption capacities toward Zn2+, Cd2+, Cu2+, Pb2+, Mn2+ or Fe3+. The results indicated that the CrIMS possessed specifically binding sites and highly selective recognition ability. However, since the IDA groups were distributed randomly in the mesoporous silica, NIMS hardly possessed selective recognition ability.
|
| Fig. 12 Selective adsorption experiments of CrIMS and NIMS (experimental conditions: initial concentrations of metal ions 1 mmol L−1, 10 mL solution at pH 4.5, 10 mg adsorbent, T = 298 K). | |
3.5. Reusability and reproducibility
Reusability and reproducibility are two nonnegligible factors in real sample treatment of adsorbents. To test the reusability, the CrIMS was used 8 times to absorb Cr(III) ions at pH 4.5. The results of experiments were presented in Fig. 13. The adsorption capacity decreased slightly after being used. The adsorption efficiency of the sample still reached 94.1% after eight cycles, proving that CrIMS possessed good reusable property. We synthesized 5 batches of CrIMS to examine the reproducibility of the adsorbents with the same synthesis method. The samples of 5 batches of CrIMS adsorbed Cr(III) ions at the concentration of 200 mg L−1 at pH 4.5. The results were displayed in Fig. 14. The related standard deviation for reproducibility ranged from 2.38% to 4.56%. The results indicated that the synthesis method can guarantee a good reproducibility of CrIMS.
|
| Fig. 13 Reusability of CrIMS (experimental conditions: 10 mL of 200 mg L−1 Cr(III) ion solution at pH 4.5, 10 mg adsorbent, T = 298 K). | |
|
| Fig. 14 Reproducibility of CrIMS (experimental conditions: 10 mL of 200 mg L−1 Cr(III) ion solution at pH 4.5, 10 mg adsorbent, T = 298 K). | |
3.6. Application of actual effluent sample
The samples of electroplating effluent were collected in polyethylene bottles from Dawang Electroplating Industrial Park (Guangdong, China) with pH 3.0 and Cr(III) ions concentration of 26 mg L−1. After the raw sample was filtered, 3.5 g of CrIMS was added into 1 L of the sample, and the residual concentration of Cr(III) ions in the solution was 0.05 mg L−1. In order to improve the adsorption capacity, the pH of water sample was adjusted to 4.5. Then, 2.6 g of CrIMS was used to adsorb Cr(III) ions from 1 L of the sample. The residual concentration of Cr(III) ions was 0.02 mg L−1. The concentrations of Cr(III) ions of the effluents after treatment were both less than the discharge standard of China (0.1 mg L−1).
3.7. Comparison with other reported adsorbents
The comparison among CrIMS and other reported adsorbents was displayed in Table 1. The simply chemistry modified materials hardly showed selectivity to Cr(III) ions. Ion imprinting technology can enhance the adsorption selectivity of adsorbents. Combined with mesoporous materials , CrIMS possessed the advantages of faster equilibrium, higher absorption capacity.
Table 1 Comparison of the reported adsorbents for Cr(III) ions
Adsorbents |
Functional groups |
Synthesis methods of materials |
Adsorption capacity (equil. time) |
Selectivity |
Ref. |
Functionalized carbon nanotubes |
Diethylenetriamine |
Chemical modification (one-step) |
5.4 mg g−1 (30 min) |
Cr, Fe, Pb and Mn |
45 |
A new chelating resin |
N-Cyclohexylacrylamide and 2-acrylamido-2-methyl-1-propanesulfonic acid |
Free radical polymerization (one-step) |
18.3 mg g−1 (−) |
Fe, Zn, Cu, Cr, Co and Mn |
46 |
Surface imprinted attapulgite sorbent |
Azodicarbonamide |
Chemical modification (multi-step) |
69.75 mg g−1 (20 min) |
Cr |
47 |
Cr(III) ion imprinted polymer grafted mesoporous SBA-15 |
Dithizone |
Chemical modification (multi-step) |
131.4 mg g−1 (−) |
Cr |
48 |
Fe3O4@ZrO2 |
— |
Sol–gel method (one-step) |
24.5 mg g−1 (7 min) |
Cr |
49 |
Imprinted polymeric beads |
Methacryloylamidohistidine |
Dispersion polymerization (one-step) |
69.28 mg g−1 (30 min) |
Cr |
50 |
Cr(III) ion imprinted polymer co-condensation modified mesoporous SBA-15 |
Iminodiacetic acid |
Sol–gel method (one-step) |
63 mg g−1 (10 min) |
Cr |
This work |
4. Conclusions
In this work, we combined ion imprinting polymers with highly ordered mesoporous silica for removal of Cr(III) ions from acidic effluents. The obtained CrIMS possessed large surface area and highly ordered pore arrays, which was the typical structure of SBA-15 mesoporous materials. Moreover, CrIMS also showed favourable selective recognition performance. The specific binding sites were distributed in ion imprinting mesoporous silica, which remarkably enhanced the accessibility for the targets and imprinted cavities. CrIMS presented higher selectivity adsorption capacity towards Cr(III) ions in an acidic solution. This effective synthesis method is convenient and can guarantee good reusability and reproducibility. In the actual treatment of effluent, the concentration of Cr(III) ions of the electroplating effluent after treatment is below the discharge standard of Cr(III) ions of China.
Conflict of interest
There are no conflicts of interest to declare.
Acknowledgements
We gratefully acknowledge the financial support from the NSFC-GD Joint Foundation of the Key Projects (No. U1201234) and National Natural Science Foundation of China (No. 21275057).
References
- Z. Zeng, L. Wang, A. Liang and J. Zhang, Electrochim. Acta, 2006, 52, 1366–1373 CrossRef CAS.
- J. Kotaś and Z. Stasicka, Environ. Pollut., 2000, 107, 263–283 CrossRef.
- Q. Duan, J. Lee, Y. Liu, H. Chen and H. Hu, Bull. Environ. Contam. Toxicol., 2016, 97, 303–309 CrossRef CAS PubMed.
- G. d. C. Cunha, J. A. Peixoto, D. R. de Souza, L. P. C. Romão and Z. S. Macedo, Green Chem., 2016, 18, 5342–5356 RSC.
- B. Zawisza, R. Skorek, G. Stankiewicz and R. Sitko, Talanta, 2012, 99, 918–923 CrossRef CAS PubMed.
- M. M. López Guerrero, E. Vereda Alonso, J. M. Cano Pavón, M. T. Siles Cordero and A. García de Torres, J. Anal. At. Spectrom., 2012, 27, 682–688 RSC.
- G. Zhang, D. Chen, W. Zhao, H. Zhao, L. Wang, W. Wang and T. Qi, Chem. Eng. J., 2016, 302, 233–238 CrossRef CAS.
- M. J. Manos and M. G. Kanatzidis, Chem. Sci., 2016, 7, 4804–4824 RSC.
- M. Zhang, L. Song, H. Jiang, S. Li, Y. Shao, J. Yang and J. Li, J. Mater. Chem. A, 2017, 5, 3434–3446 CAS.
- N. Meunier, P. Drogui, C. Montané, R. Hausler, G. Mercier and J.-F. Blais, J. Hazard. Mater., 2006, 137, 581–590 CrossRef CAS PubMed.
- G. Cimino, A. Passerini and G. Toscano, Water Res., 2000, 45, 2207–2212 Search PubMed.
- J. R. Rangel-Mendez, R. Monroy-Zepeda, E. Leyva-Ramos, P. E. Diaz-Flores and K. Shirai, J. Hazard. Mater., 2009, 162, 503–511 CrossRef CAS PubMed.
- L. Mercier and C. Detellier, Environ. Sci. Technol., 1995, 29, 1318–1323 CrossRef CAS PubMed.
- V. Ravindran, M. R. Stevens, B. N. Badriya and M. Pirbazari, AIChE J., 1999, 45, 1135–1146 CrossRef CAS.
- G. Wu, Z. Wang, J. Wang and C. He, Anal. Chim. Acta, 2007, 582, 304–310 CrossRef CAS PubMed.
- X. Jing, F. Liu, X. Yang, P. Ling, L. Li, C. Long and A. Li, J. Hazard. Mater., 2009, 167, 589–596 CrossRef CAS PubMed.
- V. K. Gupta, S. Agarwal and T. A. Saleh, Water Res., 2011, 45, 2955–2962 Search PubMed.
- R. He, W. Li, D. Deng, W. Chen, H. Li, C. Wei and Y. Tang, J. Mater. Chem. A, 2015, 3, 9789–9798 CAS.
- J. S. Beck, J. C. Vartuli, W. J. Roth, M. E. Leonowicz, C. T. Kresge, K. D. Schmitt, C. T.-W. Chu, D. H. Olson, E. W. Sheppard, S. B. McCullen, J. B. Higgins and J. L. Schlenker, J. Am. Chem. Soc., 1992, 114, 10834–10843 CrossRef CAS.
- S. Wongsakulphasatch, W. Kiatkittipong, J. Saiswat, B. Oonkhanond, A. Striolo and S. Assabumrungrat, Inorg. Chem. Commun., 2014, 46, 301–304 CrossRef CAS.
- M. Oschatz, W. S. Lamme, J. Xie, A. I. Dugulan and K. P. de Jong, ChemCatChem, 2016, 8, 2846–2852 CrossRef CAS.
- A. Bigham, S. A. Hassanzadeh-Tabrizi, M. Rafienia and H. Salehi, Ceram. Int., 2016, 42, 17185–17191 CrossRef CAS.
- Y. Du, S. Guo, S. Dong and E. Wang, Biomaterials, 2011, 32, 8584–8592 CrossRef CAS PubMed.
- A. Benhamou, M. Baudu, Z. Derriche and J. P. Basly, J. Hazard. Mater., 2009, 171, 1001–1008 CrossRef CAS PubMed.
- S. Lacasta, V. Sebastáin, C. Casado, Á. Mayoral, P. Romero, Á. Larrea, E. Vispe, P. López-Ram-de-Viu, S. Uriel and J. Coronas, Chem. Mater., 2011, 23, 1280–1287 CrossRef CAS.
- C. Tsai, Y. Pan, C. Ting, S. Vetrivel, A. S. T. Chiang, G. T. K. Fey and H. Kao, Chem. Commun., 2009, 33, 5018–5020 RSC.
- G. Vlatakis, L. I. Andersson, R. Müller and K. Mosbach, Nature, 1993, 361, 645–647 CrossRef CAS PubMed.
- D. Dechtrirat, N. G. Eichelmann, F. F. Bier and F. W. Scheller, Adv. Funct. Mater., 2014, 24, 2233–2239 CrossRef CAS.
- L. Chen, S. Xu and J. Li, Chem. Soc. Rev., 2011, 40, 2922–2942 RSC.
- L. Uzun and A. P. F. Turner, Biosens. Bioelectron., 2016, 76, 131–144 CrossRef CAS PubMed.
- L. Tan, Z. Yu, X. Zhou, D. Xing, X. Luo, R. Peng and Y. Tang, J. Chromatogr. A, 2015, 1141, 69–76 CrossRef PubMed.
- H. Niu, Y. Yang and H. Zhang, Biosens. Bioelectron., 2015, 74, 440–446 CrossRef CAS PubMed.
- L. Chen, X. Wang, W. Lu, X. Wu and J. Li, Chem. Soc. Rev., 2016, 45, 2137–2211 RSC.
- Y. Hoshino, R. C. Ohashi and Y. Miura, Adv. Mater., 2014, 26, 3718–3723 CrossRef CAS PubMed.
- Y. Chen, D. Li, Z. Bie, X. He and Z. Liu, Anal. Chem., 2016, 88, 1447–1454 CrossRef CAS PubMed.
- Y. Chen, X. Li, D. Yin, D. Li, Z. Bie and Z. Liu, Chem. Commun., 2015, 51, 10929–10932 RSC.
- X. Zheng, E. Liu, F. Zhang, Y. Yan and J. Pan, Green Chem., 2016, 18, 5031–5040 RSC.
- F. Hoffmann, M. Cornelius, J. Morell and M. Fröba, Angew. Chem., Int. Ed., 2006, 45, 3216–3251 CrossRef CAS PubMed.
- Y. Wang, L. Song, L. Zhu, B. Guo, S. Chen and W. Wu, Dalton Trans., 2014, 43, 3739–3749 RSC.
- T. Kobayashi, O. Lafon, A. S. L. Thankamony, I. I. Slowing, K. Kandel, D. Carnevale, V. Vitzthum, H. Vezin, J.-P. Amoureux, G. Bodenhausen and M. Pruski, Phys. Chem. Chem. Phys., 2013, 15, 5553–5562 RSC.
- S. Inagaki, I. Kawamura, Y. Sasaki, K. Yoshida, Y. Kubota and A. Naito, Phys. Chem. Chem. Phys., 2013, 15, 13523–13531 RSC.
- H. Liu and W. Chen, RSC Adv., 2015, 5, 27034–27042 RSC.
- T. Chang, Y. Liu, X. Yan, S. Liu and H. Zheng, RSC Adv., 2016, 6, 66297–66306 RSC.
- S. Cen, W. Li, S. Xu, Z. Wang, Y. Tang, H. Wang and C. Wei, RSC Adv., 2017, 7, 7996–8003 RSC.
- X. Zhu, Y. Cui, X. Chang and H. Wang, Talanta, 2016, 146, 358–363 CrossRef CAS PubMed.
- T. Daşbaşı, Ş. Saçmacı, N. Çankaya and C. Soykan, Food Chem., 2016, 211, 68–73 CrossRef PubMed.
- Z. Li, W. Kou, S. Wu and L. Wu, Anal. Methods, 2017, 9, 3221–3229 RSC.
- M. Jamshidi, M. Ghaedi, K. Dashtian and S. Hajati, RSC Adv., 2015, 5, 105789–105799 RSC.
- Y. Wu, J. Zhang, J. Liu, L. Chen, Z. Deng, M. Han, X. Wei, A. Yu and H. Zhang, Appl. Surf. Sci., 2012, 258, 6772–6776 CrossRef CAS.
- E. Birlik, A. Ersöz, E. Açıkkalp, A. Denizli and R. Say, J. Hazard. Mater., 2007, 140, 110–116 CrossRef CAS PubMed.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c7ra05386j |
|
This journal is © The Royal Society of Chemistry 2017 |
Click here to see how this site uses Cookies. View our privacy policy here.