G. Massaglia*ab,
A. Chiodonia,
G. P. Salvadora,
L. Delmondob,
J. A. Muñoz-Tabaresa,
S. Bocchinia,
A. Saccoa,
S. Biancoab,
G. Saraccoa and
M. Quaglio*a
aCentre for Sustainable Future Technologies@Polito, Istituto Italiano di Tecnologia, Corso Trento 21, Torino, 10129, Italy. E-mail: giulia.massaglia@iit.it; marzia.quaglio@iit.it
bApplied Science and Technology Department, Politecnico di Torino, Corso Duca degli Abruzzi 24, 10129 Torino, Italy
First published on 8th August 2017
This work investigates the effect of nanofiber/nets (NFN) on the electrical behaviour of conductive composite nanofibers, using polyethylene oxide (PEO)/multiwall carbon nanotubes (MWCNT) as the model material for the analysis. We demonstrate that water-based solutions, containing high molecular weight PEO and MWCNT can be processed by electrospinning/netting applying high voltages. NFNs are designed with different morphologies, in particular modulating their porosities. A strong enhancement of the electrical conductivity of PEO/MWCNT–NFN is observed for the denser NFN, if compared to nanofiber composites. These results demonstrate that the NFN morphology can directly control the quality of the electron percolation paths. To provide better evidence for this strong dependency we processed the nanocomposite NFN by solvent-induced swelling. This physical mechanism directly modulates the percolation path, tuning the electrical behaviour of the nanocomposites to a resistive one: the better the starting percolation path, the larger the resistivity increase.
In this paper we describe the nanocomposite obtained by adding multiwall carbon nanotubes (MWCNTs) to a water-based solution of polyethylene oxide (PEO). Sodium polystyrene sulfonate (Na-PSS) was chosen as surfactant agent, as reported in former works on MWCNTs,15–17 in order to effectively dispersed MWCNT in the initial solution and in the following products. The resulting fibrous nanocomposite was the model material to investigate the behaviour of electrically conductive NFN-nanocomposites. The electrical properties of PEO/MWCNT nanofibers have been deeply investigated by McCullen et al.,18 demonstrating that the MWCNT concentration directly modulates the electrical conductivity, according to the percolation model. In this kind of composite material, the actual morphology of the polymer nanofibers hosting the conductive filler can strongly influence the creation of efficient percolation paths; therefore the presence of NFN can deeply modify its electrical behaviour.
We firstly demonstrate the possibility to obtain NFN by electrospinning/netting of PEO/MWCNT nanocomposite, proving that they can form when using high molecular weight PEO and high voltages. By controlling the process parameters, we obtained different morphologies of the NFN, especially in terms of density and shape of nanonets.
We then analysed the electrical behaviour of PEO/MWCNT–NFN, confirming the validity of the percolation model in this system. We demonstrated that the morphology of the NFN system deeply influences its electrical behaviour, showing also the possibility to modulate the percolation path in NFN nanocomposites, by exploiting the effect of solvent (water)-induced swelling. Indeed, by swelling PEO-based nanofibers and nanonets with water, we changed their average diameters, thereby increasing the average distance among MWCNTs. This physical mechanism directly enhances the resistive behaviour of the nanocomposite: the better the starting percolation path, the larger the resistivity increase.
Aluminum foils were used as the reference substrates during process optimization. Samples for TEM analysis were prepared by directly electrospinning the nanofibers on a standard holey carbon Cu TEM grid.
Glass slides were used as substrates to fabricate the samples for electrical characterizations. Hard-masks, made of poly(methyl)methacrylate were fabricated by column drill, and used both to prepare the electrodes and to shape the nanofibers mats for the characterizations. Strips of nanofibers were prepared, having a length of 2 cm and a width of 2 mm. The thickness of the nanofiber strips was evaluated by a Tencor P-10 Surface Profiler and confirmed by FESEM analysis on samples analysed in cross-section. Four platinum electrodes were obtained for each nanofiber strip, using a hard mask during sputtering from a Pt target, applying a current of 50 mA for 120 s (Q150T ES by Quorum Technologies). The resulting platinum films were 100 nm thick, 1 mm wide and 5 mm long. The four-points electrical characterizations were performed by polarising the samples, applying different values of electrical potential difference (V), and measuring the resulting current (I) flowing through the sample by means of a Keithley 2635A Source measure unit.
In the present work, we promoted the electrospinning/netting process by adding high molecular weight (Mw) PEO to a water-based solution containing PSS-functionalized MWCNTs, and by applying high voltages during the electrospinning process.
The detailed composition of all the solutions tested in this work, as well as their electrical conductivities and rheological behaviour, are listed in Table S-1 in the ESI.† We obtained ESN process using PEO with the highest molecular weight (i.e., 1000 kDa) at the highest concentration (i.e., 5 wt%). No nanonets were observed for lower working parameters, as reported in the Fig. S3† in the ESM. The name of the nanocomposite samples has the general structure PEO-x-y@z, where x is the polymer Mw, y refers to the amount of MWCNTs and z refers to the voltage applied during the electrospinning process. When a class of samples with different concentrations of MWCNTs is considered, a specific value will not be assigned to y.
We hypothesized that the ESN is promoted by the combined effect of Na-PSS additive and high molecular weight PEO. In Fig. 1 the PSS is simplified by a pink line with negative charges: when Na-PSS is added to MWCNTs in water, PSS links to the MWCNT surface, exposing the negative charges, well balanced by the Na+ ions, to water, as proposed in Fig. 1(a). By adding PEO to the solution, Na+ are attracted by the ether groups. The resulting mobility of positive and negative charges into the final polymeric solution is reduced. When the electric field is applied, the polymeric solution at the tip of the needle can expose unbalanced local concentration of the positive Na+ ions linked to the PEO ether groups, and the negatively charged PSS–MWCNTs, so increasing the probability of charge unbalances inside the nanofibers, as sketched in Fig. 2(a). Interestingly, when PEO with a molecular weight of 600 kDa is used, no NFNs form, even if using high voltages (see Fig. S-3a† in the ESM). When the molecular weight is increased to 1000 kDa, NFNs form, with a structure that becomes more complex for increasing values of the applied voltage and for higher concentration of Na-PSS/MWCNTs, as shown in Fig. 2(b). Therefore, we suggest that the use of high Mw is critical to favour random, unbalanced distribution of charges, and then to form NFN, as proposed in Fig. 2(a). Indeed, it is important to consider that, thanks to the high number of entanglements present in the high Mw PEO, it is quite easy to create charge unbalances by the reduced ion mobility during the fast ESN process.
Different net charge distributions between adjacent nanofibers can significantly contribute to the creation of strong local secondary electric fields that can generate the secondary nanofiber net, as sketched in Fig. 2a. The result is the formation of nanofiber/nets, according to a mechanism similar to that proposed by N. A. M. Barakat et al.,9 based on the effect of salt additives.
In order to analyse the actual distribution and the orientation of MWCNTs inside the nanofibers-net, and to gain a better understanding of the morphology of the PEO/MWCNT-NFN, TEM analyses were performed. We selected 23 kV and 0.1 ml h−1 as the reference electrospinning parameters and fixed the MWCNT loading at 1.5 wt%. Nanofiber/nets were directly collected on standard holey carbon TEM Cu grid. Fig. 2(c) and (d) help to confirm that the MWCNTs are aligned along the main axis of the nanofibers, showing the presence of MWCNTs even in small-size nanofibers.
The morphology of the NFNs obtained for the nanocomposite samples are shown in Fig. 3. FESEM pictures of samples PEO-1000-1.5@18 and PEO-1000-1.5@23 are shown in Fig. 3(a) and (b) respectively, while samples PEO-1000-3.5@18 and PEO-1000-3.5@23 are shown in Fig. 3(c) and (d), respectively. The NFNs are highlighted in yellow, showing the creation of a secondary web, made of very small-size nanofibers. By increasing the voltage up to 23 kV and the MWCNT concentration up to 3.5 wt%, the nanofiber-net morphology becomes more complex. Indeed, the comparison of the first line with respect to the second line of Fig. 3, makes it clear that the nanofiber nets are denser in the composite systems having a higher content of MWCNTs, meaning that more nanonets form connecting the main nanofibers, occupying the inner pores of the material. This observation is consistent with the hypothesis that MWCNTs rule the NFN creation process. Comparing the first column of Fig. 3 to the second one, the effect of increasing values of the working voltage is appreciable, especially showing the formation of nanobeads, distributed along the nanonets, as shown in Fig. 3. We will refer to this structure as nanobeaded-NN. The concentration of nanobeaded-NN increases both with the concentration of MWCNTs and the applied voltage.
We consider MWCNTs to play a key role in determining the nanobeaded morphology of the PEO/MWCNT–NFN. As already investigated in electrospinning,21 beads can form during the travel of the fluid jet, if the driving force elongating the nanofiber is reduced. Thus, we suggest that unbalanced charges, due to MWCNTs, alter the actual electrical field applied to the nanofibers, so favouring the creation of nanobeaded-NN as evidenced by the TEM analysis reported in Fig. 2(d).
A percolation behaviour has been demonstrated by McCullen et al. for the PEO/MWCNT nanofiber composite.18 To investigate the role of nanonets on the electrical behaviour of the PEO/MWCNT–NFN nanocomposite, some samples were fabricated using solutions made of both a low and a high PEO molecular weights (i.e., PEO-600 and PEO-1000 samples, respectively), with different mass fractions of MWCNTs. Since no NFN has been observed in PEO-600 samples (as proposed in the ESI†), we selected them as the reference to show the electrical behaviour of standard NF, comparing them with the NFN samples obtained using the 1000 KDa PEO. Moreover, PEO-600 samples were processed at 18 kV only, while the PEO-1000 samples were fabricated at two different voltages, i.e. 18 and 23 kV, in order to obtain samples with different nanonets densities, as reported in Fig. 3.
The experimental values of the electrical conductivity as a function of the MWCNT weight percentages are represented in Fig. 4(a). We fitted the three sets of data with the percolation models reported in eqn (1) and (2), that describe the electrical conductivity as a function of the filler content above and below the percolation threshold, respectively.
σ = σ0(p−pc)s | (1) |
σ = σd(pc−p)t | (2) |
In the model, pc is the percolation threshold, σ is the electrical conductivity, p is the weight percentage of MWCNTs, and σ0, σd, t and s are fit parameters. The fitting curves are proposed in Fig. 4(a), and the resulting values of the percolation thresholds, pc, are highlighted in same figure. The minimum pc value of 1.5 wt% was found for samples PEO-600@18, while higher values of 2.2 and 2.1 wt%, were estimated for samples PEO-1000@23 and PEO-1000@18, respectively.
It is interesting to notice that: (1) pc increases for increasing values of the polymer average molecular weight; (2) for each MWCNT concentration, the conductivity of PEO-1000@18 is lower than the conductivity of the PEO-600@18 samples; (3) the PEO-1000@23 curve reaches the highest values of conductivity above percolation among the three set of samples. The latter two behaviours can be explained by comparing the morphology of the different samples.
In Fig. 4(a), two sets of FESEM images are proposed as inserts: they show the nanofibers and nanofiber/nets obtained for the three groups of samples, both at 1.5 wt% and at 3.5 wt% of MWCNTs. Comparing the images of nanofibers from samples PEO-600-1.5@18 and PEO-600-3.5@18 (with the green frames) to the pictures referring to the PEO-1000-1.5@18 and PEO-1000-3.5@18 nanofiber/nets (blue frames), it can be noticed that the latter samples show a nanofiber/net structure with a very low density (as described also in the ESM, Fig. S-3†), with less NFNs occupying pores than those visible in the PEO-600@18 samples. In this case, the presence of low-density NFN is detrimental for the creation of percolation paths, since the distance among nanofibers is higher than for the other samples, so that higher concentration of MWCNTs are necessary to reach the percolation threshold. Moreover, above the percolation threshold, for each concentration of MWCNTs, the electrical conductivity remains lower than that of samples made with standard NF, thus demonstrating difficult electron transfer process among carbon nanotubes.
The PEO-1000@23 samples (red curve in Fig. 4(a)) exhibit a completely different electrical behaviour than the PEO-1000@18 samples. Again we consider the morphology of the nanostructured materials to play a crucial role: indeed the former samples, processed at higher voltage show a more compact NFN structure, as shown in the pictures inserted in Fig. 4(a) with a red frame. In particular, by increasing the amount of MWCNTs in the material, pores are progressively occupied by NN and nanobeaded-NN. In addition, MWCNTs are present also in very small-size nanofibers, even in the secondary nanoweb, as shown in Fig. 2(d). This turns in the progressive improvement of the percolation networks while increasing the MWCNT content, thus increasing the probability of charge transfer across the mat of nanofibers, also thanks to the contribution of the nanonets. The result is that dense NFNs exhibit the onset of the electrical percolation at MWCNT concentration close to the value found for the less dense NFN, but the electrical conductivity above percolation is significantly improved. As a consequence, the final electrical behaviour of electrospinning-based composites can be tuned not only selecting its composition, by also by a careful design of the final nanostructure.
The designed material demonstrates new intriguing possibilities to optimize the NFN systems, in order to tune their morphology as well as their functional behaviour to match different potential application areas, as tissue engineering and environmental sensing. In both fields, the direct combined control of electrical conductivity and surface area of nanostructured mats can play a crucial role to gain optimal performance.22–25 With the aim to emphasize the potentiality of the NFN functional composite material, with unique morphological characteristics, properly combined with its tailored conduction properties, we performed preliminary tests to analyse its behaviour when exposed to humidity, investigating the effect of solvent-induced swelling on the conductivity.
The NFN functional composites designed in this work can be classified as conductive polymer composites,25,26 made of a polymeric matrix (i.e. the NFN) hosting an electrically-conductive filler. Exposure to humidity is expected to cause the polymeric nanofibers and NFN to swell by water adsorption, so increasing the distance among MWCNTs: if the concentration of MWCNTs is above the percolation threshold, the polymer swelling can directly affect conduction. Moreover, the worse is the quality of the percolation network, the lower will be the response of the material to the effect of swelling.
We performed the tests using the same sample architecture already used for the electrical characterizations of the material, directly exposing them to a vapour flow in air, generated by an aerosol system placed in proximity of the sample. We selected an aerosol system to avoid any effect of temperature on the samples during the tests. We worked at room temperature (i.e., 23 °C) and the lowest value of the relative humidity was the ambient one (i.e., 23% RH). A digital thermo-hygrometer (DTH) was placed in close proximity of the sample under investigation: 30 s were necessary to change the relative humidity from the lowest (23% RH) to the highest (60% RH) value, according to the DTH; after that time the humidity remained constant at 60% RH. Vapour was supplied to the sample in cycles: 30 s of exposure to humidity followed by 2 minutes of no exposure, working as a resting time necessary to restore the behaviour of the nanostructured samples to that shown before exposure to humidity.
The results are shown in Fig. 4(b), reporting the dimensionless relative differential resistance, ΔR/R0 as a function of time. ΔR/R0 is defined in eqn (3)
ΔR/R0 = (R−R0)/R0 | (3) |
The overall results are impressively in line with the expected behaviour of these systems. Indeed, samples PEO-1000-3.5@23 with a dense NFN structure, show a better behaviour than samples with NF only, because of the improved percolation pathways, giving higher electrical conductivity above percolation threshold. Dense NFN of PEO-1000-3.5@23 samples had a 4 times higher value of ΔR/R0 than samples PEO-600-3.5@18 with standard NF mats.
Analysing the curves in Fig. 4(b), the recovery speed (Rs) can be introduced, to help describing how fast the material regain its initial state after perturbation with humidity. Rs can be evaluated as the slope of the curves in the descendant part of each cycle. Analysing the materials by this approach, samples PEO-1000-3.5@18 and PEO-1000-3.5@23 show the fastest recovery process, with an average speed of 0.17 s−1 and −0.14 s−1, respectively, while PEO-600 samples exhibit a quite slower recovery process, with an average Rs of −0.05 s−1. This means that the NFNs, both the more and less dense one, help to improve the recovery process, and this can be explained considering that the nanowebs exhibit lower diameters than conventional NF mats. This turns in a faster humidity removal, that corresponds to a faster restoring of the percolation paths.
These results show that the electrical behaviour of composite NFNs can be directly tuned by the proper design of the nanonetting morphology, demonstrating a great potential of NFN composite materials.
The electrical behaviour of the resulting PEO/MWCNT–NFN composite was analysed. The percolation theory was successfully applied, and a significant increase of the electrical conductivity was noticed, when a dense NFN was present in the material.
To investigate the direct effect of morphology on the final electrical behaviour of composite NFN, the response of the material to humidity-induced swelling was evaluated. Dense NFN significantly amplify the response of the material to external water vapour stimulus. The relative differential resistance of the denser NFN was four times higher than that shown by the standard composite NF. Moreover the recovery process was quite faster.
That experiment definitely demonstrated that the electrical behaviour of MWCNT based composite NFNs can be directly tuned by the proper design of the nanonets morphology.
Moreover, this tunable functional behaviour, when coupled to the biocompatibility and safety of PEO, results in a new amazing set of properties of the PEO/MWCNT–NFN, with great potential in fields as environmental sciences and tissue engineering.
Footnote |
† Electronic supplementary information (ESI) available: Describing the properties of starting solutions, the selection of the polymer concentration, the results of Raman spectroscopy, and comparing the morphology for standard nanofibers and nanofiber/nets is available. See DOI: 10.1039/c7ra05573k |
This journal is © The Royal Society of Chemistry 2017 |