Yuying Zhenga,
Peishan Hea,
Yanxiong Fanga,
Xu Yang*b and
Huagen Liang*c
aSchool of Chemical Engineering and Light Industry, Guangdong University of Technology, Guangzhou 510006, China
bGuangzhou Institute of Energy Conversion, Chinese Academy of Sciences, Guangzhou 510640, China. E-mail: yangxu@ms.giec.ac.cn; Tel: +86-020-87057620
cLow Carbon Energy Institute, School of Chemical Engineering & Technology, China University of Mining and Technology, Xuzhou, 221116, China. E-mail: lhg654@gmail.com; Tel: +86-0516-83883501
First published on 20th June 2017
Selective hydrogenation of phenol is of great significant for the production of Nylon 6. Herein, highly efficient and stable Ir promoted Pt catalysts for the hydrogenation of phenol are prepared by deposition of Pt–Ir nanoparticles onto hollow mesoporous silica spheres (HMSs) through a facile wet-impregnation and H2 reduction method. The obtained PtIr/HMS catalyst with Ir/Pt molar ratio of 0.1 shows a highest hydrogenation rate of 4255 mmol h−1 gPt−1 with cyclohexanone selectivity of 85% at 50 °C and 0.5 MPa of pH2, which is 3 times and 8.6 times higher than that of the mono Pt/HMS catalyst and commercial Pt catalyst, respectively. The trace addition of Ir promoter essentially contributes to the enhanced hydrogenation activity by improving the metal dispersion of Pt nanoparticles and promoting the charge transfer between the Pt and Ir. This work provides an effective protocol in developing high performance catalysts for phenol hydrogenation under mild reaction conditions.
A lot of research work on the development of the catalyst has been reported in the last decade.5–10 Current prevailing catalysts used for hydrogenation include Ni and Pd supported catalysts; the former ones are often operated under rigorous reaction conditions (T > 200 °C or pH2 > 1 MPa),11,12 the latter are confronted with severe metal sintering and leaching that often lead to deactivation issues.2,5,6 Noticeably, the Pt based catalysts exhibit excellent activity and stability under mild reaction conditions.9,13,14 However, one major obstacle for practical application of Pt based catalysts is their scarce reserves and high cost. Therefore, several strategies have been tried to increase the Pt utilization efficiency, such as core–shell composites,15,16 Pt monolayer catalysts,17,18 alloying with other metals,19 adding promoter,20,21 etc.
Of these protocols, adding promoter is both economically and effectively method due to its simple procedure and convenient controlling. Moreover, literatures elsewhere have envisioned that trace promoter not only can remarkably enhance the activity, but also tune the selectivity for various chemical reactions. For example, Tomita and co-authors have reported that addition of iron oxide can effectively improve the activity of Pt/Al2O3 towards CO oxidation.22 Burch et al. have investigated a series of Pt/Al2O3 catalysts promoted by metal oxides or noble metals (Ag, Au, Pd, Rh) for the NO reduction, claiming that the promoters have a significant effect on the activity of Pt/Al2O3.21 Luo and co-authors have found that the Ir promoted Ru/ZnO showed high selectivity towards crotyl alcohol applied in crotonaldehyde hydrogenation.23 They ascribed the improved selectivity to the modified electronic properties of Ru induced by the Ir promoter. These reports demonstrate well that high performance catalyst can be achieved as the promoters are elegant selected.
In this work, we attempt to obtain a high-performance Ir promoted Pt bimetal catalysts for selective hydrogenation of phenol. To the best of our knowledge, the promotion effect of Ir on the Pt towards phenol hydrogenation has seldom been reported. Previously, we have used our lab-made hollow mesoporous silica (HMS) as support of Pd catalyst for phenol hydrogenation.24 With high surface area (∼800 m2 g−1) and narrowed mesopores, the HMS can effectively disperse the Pd components. Moreover, the HMS can exert its inactive siliceous properties as an ideal candidate to investigate the promoter effect with less interruption by metal-support interaction. Thus, we herein selected the HMS as support to prepare PtIr/HMS catalysts with various molar ratio of Ir/Pt through impregnation and reduction route. The effect of promoter on the Pt based catalysts was investigated comprehensively as to explore the Pt–Ir synergy effect on the performance towards hydrogenation of phenol.
Pt–Ir bimetallic catalysts with various molar ratio of Ir/Pt (from 0 to 0.2) were prepared according to a wet-impregnation and H2 reduction route. Firstly, 1.0 g HMS supports were impregnated with 20 ml ethanol solution of chloroplatinic acid (0.03 g) and chloroiridic acid (0–0.008 g) with given molar ratio, and kept stirring at room temperature. The solvent was then evaporated in a water bath at 50 °C. The PtIr/HMS catalysts were finally prepared by reducing the sample under hydrogen flow at 300 °C for 4 h in a tubular furnace with programmed temperature control, at a rate of 2 °C min−1. The Pt loading was fixed at 1.5% for all catalysts, and the basic specifications of catalysts are listed in Table 1. A commercial Pt/C catalyst was purchased from Aladdin agent Company for reference sample.
Catalyst | SBETa (m2 g−1) | DPorea (nm) | Metal loadingb | DPtc (nm) | |
---|---|---|---|---|---|
Pt wt% | Ir wt% | ||||
a Surface area (SBET) and pore size (DPore) were derived from the iso-thermal nitrogen ads–desorption curves.b Metal loading was determined by ICP measurement.c Average particle size of Pt crystallite (DPt) was calculated from the XRD plot according to the Scherrer equation. | |||||
HMS | 837 | 3.7 | — | — | — |
Pt/C | 56 | — | 5 | — | 4.2 |
Pt/HMS | 821 | 3.3 | 1.50 | — | 3.8 |
PtIr0.05/HMS | 806 | 3.5 | 1.52 | 0.07 | 3.4 |
PtIr0.1/HMS | 812 | 3.5 | 1.48 | 0.16 | 3.2 |
PtIr0.2/HMS | 809 | 3.4 | 1.50 | 0.31 | 3.0 |
![]() | ||
Fig. 1 Small angle XRD patterns (a) and isothermal N2 adsorption–desorption plot (b) of the calcined HMS materials. |
Fig. 2 shows the wide-angle XRD patterns to characterize the metal crystallites of the catalysts. A broaden peak centred at 24° of 2θ is observed for all samples, which is ascribed to the amorphous silica. The Pt/HMS exhibits three clear diffraction peaks located at 39.4, 46.1 and 66.9° of 2θ, indexing to the (111), (200), and (220) planes of the face-cantered cubic Pt crystallite.27 With the addition of Ir promoter, such three peaks become broadened and diminished, suggesting that the Ir promoter can weaken the crystalline degree of Pt, or improve the metal dispersion. From the enlarged regional XRD between 30 and 50°, the half width of (111) peaks increase upon the Ir addition elevated. Table 1 presents the crystallite size calculated by the Scherrer equation. The particle size decreases from 3.8 to 3.0 nm as the molar ratio of Ir/Pt increase from 0 to 0.2. It is clear that the addition of Ir promoter plays a crucial role for enhancing the dispersion and decreasing the particle size of Pt components.
![]() | ||
Fig. 2 Wide angle XRD pattern (a) and enlarged region between 30 and 50° of 2θ (b) for PtIr/HMS catalysts with various Ir/Pt molar ratio. |
Fig. 3 presents the TEM images of the mono-Pt/HMS and PtIr0.1/HMS catalysts for comparison. It verifies the micro-structure of hollow cavity and mesoporous shell for the HMS support. In addition, the highly dispersion of active components on the HMS is seen clearly as well. The mono-Pt/HMS shows some poly-dispersed Pt nano-particles on the mesoporous shell (Fig. 3b), while the PtIr0.1/HMS presents homogeneously dispersed Pt nano-particles (Fig. 3d), further confirming the promotion effect of Ir on the metal dispersion.
To determine the crystallite size and lattice fringe of Pt nano-particles precisely, the high-resolution TEM was conducted for these samples. As shown in Fig. 4, the PtIr0.1/HMS has a smaller particle size (∼2 nm) than that of the Pt/HMS (∼4 nm). Moreover, in the corresponding diffraction patterns, the PtIr0.1/HMS exhibits less of diffraction light spots than the Pt/HMS does, implying its less crystalline degree or smaller particle size, consistent with the XRD analysis. The (111) inter-planar distances derived from the diffraction pattern, indicate 0.218 and 0.228 nm for PtIr0.1/HMS and Pt/HMS, respectively, further revealing the contraction of Pt unit cell upon the addition of Ir. This can be associated with the formation of PtIr alloy.28,29 It demonstrates well that the addition of Ir promoter can result in the formation of PtIr alloy, and improve the metal dispersion.
H2-TPR profiles of the as-prepared catalysts after impregnation are presented in Fig. 5. The Pt/HMS exhibits a strong sharp peak located at approximately 117 °C, attributable to the easy reducible Pt2+ ions. The PtIr0.1/HMS and PtIr0.2/HMS show a relative high temperature reduction peak centred at 177 and 191 °C, respectively, which implies the hard reducible bimetal species on the catalysts. This can be ascribed to the strengthened interactions between the Pt precursors and silica,9 or to the formation of PtIr alloy. It demonstrates that the addition of Ir can intensify the metal support interaction, which would modulate the electronic properties of Pt phase.
Fig. 6 shows X-ray photoelectron spectroscopy (XPS) of samples to assess the surface information of metal states and compositions. The Pt 4f spectra can be fitted by two doublets attributed to the higher binding energy of Pt2+ (73.2–73.8 eV) and lower energy value of metallic Pt0 (71.9–72.2 eV).30 Compared with the Pt/HMS catalysts, a shift of ∼0.3 eV towards high energy occurred for the bimetal PtIr0.1/HMS catalysts, indicating the electronic properties of Pt can be modulated by the Ir promoter. In addition, the XPS derived Pt0/Pt2+ atomic ratio indicates that the PtIr0.1/HMS held more of metallic Pt phase than the Pt/HMS has, suggesting the Ir promoter can resist the re-oxidation of metallic Pt species. It further verifies the modulation of electronic properties of Pt caused by the Ir promoter. The Ir 4f spectrum (Fig. 6c) indicates the 4f7/2 and 4f5/2 peaks at binding energy of 61.0 and 64.1 eV, respectively, assigning to the metallic state of Ir phase.31 The well-defined peak centred at 103.8 eV is observable for both samples, corresponding to the 2p binding energy of silica.
![]() | ||
Fig. 6 XPS spectra of various catalysts: (a and b) Pt 4f, (c) Ir 4f and (d) Si 2p in Pt/HMS and PtIr0.1/HMS. |
Further increases the Ir addition, the conversion of PtIr0.2/HMS shows a slight decline at 55%. These results demonstrate that the Ir promoter could remarkably enhance the phenol hydrogenation activity; the optimum molar ratio of Ir/Pt is 0.1. The recycle test was conducted for the PtIr0.1/HMS, as shown in Fig. 7b. After fourth run, it exhibits slight decline of conversion (<2%), accompanied with constant selectivity of 84% towards cyclohexanone. The TEM images of spend catalyst (seeing Fig. S1 in ESI†) after hydrogenation suggested negligible metal sintering, demonstrating the good stability of for the PtIr0.1/HMS catalyst.
Several limitations of the current catalytic system, such as harsh reaction conditions, deactivation and etc., have driven scientists to develop high-performance catalysts applied in mild reaction.7,25,32 Compared with the methods in documents elsewhere,5,6,10–14 the high activity and good stability of the PtIr/HMS make it one of promising catalysts applied for phenol hydrogenation in mild reactions.
The influence of reaction temperature on the PtIr0.1/HMS was investigated, as shown in Fig. 8a. As the temperature is elevated from 30 °C to 100 °C, the phenol conversion soars from 15% to 100%. However, the selectivity of cyclohexanone decreases upon the increase of temperature, implying high reaction temperature facilitates deep hydrogenation of cyclohexanone to cyclohexanol. It reveals that the PtIr0.1/HMS is suitable for production of cyclohexanone through phenol hydrogenation under mild reaction. Based on the activity upon the reaction temperature, we plotted the Arrhenius curves for the Pt/HMS and PtIr0.1/HMS, as depicted in Fig. 8b. The apparent activation energy was 39.5 and 31.4 kJ mol−1 for Pt/HMS and PtIr0.1/HMS, respectively, further verifying the promotion effect of Ir on the Pt.
Footnote |
† Electronic supplementary information (ESI) available: Catalyst characterizations, schemes for reaction pathway and mechanistic proposition of phenol hydrogenation. See DOI: 10.1039/c7ra05653b |
This journal is © The Royal Society of Chemistry 2017 |