Dong Ding,
Bo Zhou,
Shurong Liu,
Guijie Zhu,
Xianwei Meng,
Jiandong Yang,
Wuyou Fu and
Haibin Yang*
State Key Laboratory of Superhard Materials, Jilin University, Changchun 130012, P. R. China. E-mail: yanghb@jlu.edu.cn; Tel: +86 431 85168763
First published on 25th July 2017
In this study, we report a TiO2 hybrid structure prepared by a facile route, wherein TiF62− ion has been used as both the surfactant and titanium source. Single-crystalline TiO2 nano-polyhedrons with exposed high active {001} facets were grown on a TiO2 nanowire and nanotube (TWTs) films. This hybrid structure served as a model architecture for efficient photoelectrochemical (PEC) devices because it simultaneously offered a large contact area with the electrolyte and direct pathway for photoexcited electron collection. Under simulated sunlight illumination (AM 1.5 light at 100 mW cm−2), this hybrid structure exhibited a photocurrent density of 1.36 mA cm−2 at 0 V vs. Ag/AgCl (JSC) and photoconversion efficiency (η) of 0.81% at −0.51 V vs. Ag/AgCl, nearly 2.4 times higher than those of the bare TWTs. Morphology of the TiO2 nano-polyhedrons in the hybrid structure was greatly influenced by the TiF62− ion concentration, and a proper concentration was determined to be 2.5 mM. Moreover, the CdS QDs were sensitized onto the hybrid structure, and their JSC and η reached 2.31 mA cm−2 & 1.94%, respectively, 1.5 times higher than those of the CdS-sensitized bare TWTs. The TiO2 nano-polyhedrons improved the efficiency via increasing the specific surface area of the electrode, thus facilitating hole transfer into the electrolyte. Moreover, the exposed high reactive {001} facets provided more effective area for the adsorption of CdS, leading to an enhanced photogeneration carrier density.
Moreover, PEC performance of TiO2 is closely associated with its exposed facets; theoretical and experimental studies reveal that the {001} facets achieve higher chemical activities than {101} and {100} facets in the anatase TiO2 crystals (the average surface energies of anatase TiO2 are in the order γ {001} (0.90 J m−2) > γ {100} (0.53 J m−2) > γ {101} (0.44 J m−2)).19 This can be attributed to the larger Ti–O–Ti bond angle on the {001} facets, which make the 2p states of the surface O atoms unstable and very reactive.20 However, according to the Wulff construction, the {001} facets tend to diminish during the free crystal growth process to minimize the total surface energy.21,22 Surfactant-assisted method is a popular approach for the controlled synthesis of {001} facet-exposed anatase TiO2, in which F− are introduced as surfactants.23,24 Lu et al. used TiF4 and HF as raw materials in a Teflon-lined autoclave to prepare {001} facet-exposed TiO2 single crystals and found that the {001} facets played crucial roles in photoreactivity improvement of TiO2.25,26 Pan et al. have prepared N + Ni co-doped anatase TiO2 nanocrystals with exposed {001} facets using a two-step hydrothermal reaction, and the as-prepared sample showed a superior photocatalytic activity.27 The synthesized TiO2 single crystals and TWT hybrid structure with highly reactive {001} facets can have potential applications in several areas such as in photocatalytic CO2 reduction, solar cells, and photonic and optoelectronic devices.
In this study, we synthesized a novel TiO2 hybrid structure via a facile route, as illustrated in Scheme 1. First, highly ordered TiO2 nanotubes and nanowires (TWTs) on a Ti foil were prepared by electrochemical anodization. Second, single-crystalline TiO2 nano-polyhedrons with exposed {001} facets were grown on TWTs through a chemical bath deposition (CBD) process under atmospheric pressure, wherein TiF62− was used as both the surfactant and titanium source. We conducted varied TiF62− concentration studies during the CBD process and proposed a possible growth mechanism. Third, CdS QDs were assembled onto bare TWTs and hybrid structure via successive ionic layer adsorption and reaction (SILAR) technique. CdS (Eg ≈ 2.4 eV) sensitization is considered as an effective method to broaden the solar absorption spectrum of TiO2 (Eg ≈ 3.2 eV). Thus, we obtained a hybrid structure with superior PEC performance than bare TWTs owing to its preponderances of increased surface area and exposed highly reactive {001} facets.
PEC performance of the samples was analysed via an electrochemical workstation (CH Instruments, model CHI601C) using a Ag/AgCl reference electrode and a Pt wire as the counter electrode. A 500 W Xe lamp (Spectra Physics) with a monochromator simulated sunlight, which was adjusted to provide AM 1.5 light at 100 mW cm−2 using a laser power meter (BG26M92C, Midwest Group). The electrolyte solution consisted of 0.25 M Na2S·9H2O, 0.35 M Na2SO3, and 0.1 M KCl aqueous solution (pH = 12). The photoconversion efficiency (η) was calculated from the line sweep voltammogram as follows:28,29
η = JSC(Eo − E)/I |
The IPCE of the samples were measured using a two-electrode system with an action spectrum measurement setup (PEC-S20, Peccell Ltd.). Before the measurement, the samples were sealed in sandwich structures with a 60 μm spacer using Pt as the counter electrode. The electrolyte was injected between the two electrodes. Light was irradiated from the counter electrode side.
Fig. 1 SEM images (A and B), HRTEM and FFT images (C and D), and XRD pattern (E) of hybrid structure. |
In a typical anodizing system, Ti is corroded into TiF62− by F− under electric current; thereafter, TiF62− hydrolyses into Ti(OH)4, and the stacking blocks of the nanotube. Then, the nanotubes undergo an annealing process in which Ti–O–Ti are joined via dehydration. When the sample is merged into the TiF62− solution, TiO2 nucleates on nanotubes and grows into nano-polyhedrons. Fig. 2 and S3† show the SEM images of the samples synthesized at the TiF62− concentration of 0.5 mM, 1.5 mM, 2.5 mM, and 3.5 mM (denoted as S-0.5/1.5/2.5/3.5, respectively). As TiF62− concentration increases from 0.5 mM to 2.5 mM, the grain size of the polyhedron increases from 22.5 nm to 91.5 nm and the shape becomes regular. We deduced that the TiO2 nano-polyhedrons were formed through the hydrolysis of TiF62− through the following reaction:
[TiF6]2− + nH2O ↔ [Ti(OH)nF6−n]2− + nHF |
[Ti(OH)6]2− + 2H+ → TiO2 + 4H2O |
Fig. 2 SEM images of the hybrid structure synthesized at varied TiF62− concentrations: 0.5 mM (A), 1.5 mM (B), 2.5 mM (C), and 3.5 mM (D). Schematic showing the TiO2 nano-polyhedron formation (E). |
Usually, TiO62− octahedra are the building blocks of TiO2. As illustrated in Fig. 2E, F− generated by hydrolysis process could favorably adsorb on the high active {001} facets of TiO2 and suppress the growth along the [001] direction. Consequently, the resulting TiO2 crystal nucleus maintains the {001} facet-exposed truncated octahedral structure.25 When the TWTs are immersed in TiF62− solution, TiO2 nucleates on TWTs and grows into nano-polyhedrons. When the TiF62− concentration increases, the surface of these {001} facets-exposed TiO2 crystal nucleus hydrolyzes and F− would be replaced by hydroxyl groups; then, the oriented adsorption process occurs under the influence of dehydration condensation reaction between hydroxyl groups. Hence, the size of the TiO2 nano-polyhedrons becomes larger. This indicates that at this stage, the TiF62− concentration is the main parameter affecting the growth of the polyhedrons; as the TiF62− concentration increases, the system can afford enough growth dynamic to gradually form an entire (001) low-energy surface. However, when the TiF62− concentration further increases to 3.5 mM, the grain size remains ∼91 nm, but the surfaces become rough. This can be attributed to further nucleation on the polyhedron surfaces caused by extreme undercooling.
PEC performance of the hybrid structure samples prepared at different TiF62− concentrations is shown in Fig. S6.† The S-2.5 sample shows the best PEC performance owing to the greater specific surface area and exposed {001} facets. On the other hand, when the TiF62− concentration reaches 3.5 mM, randomly deposited TiO2 crystal nuclei on the nano-polyhedrons cover the high active {001} facets and result in a decreased JSC and η. In this study, the S-2.5 sample has been chosen for the following CdS QD sensitization investigation. The CdS QD-sensitized bare TWTs were prepared and investigated for comparison.
The as-prepared hybrid structure samples were further sensitized by CdS QDs, as shown in Fig. 3. Fig. 3A and B show the top- and side-view SEM images. The surfaces of the arrayed TWTs and nano-polyhedrons are decorated by evenly distributed CdS QDs and become rough. Moreover, the CdS QDs on the TWTs and nano-polyhedrons are investigated by HRTEM, as shown in Fig. 3C and D, respectively. The average size of the CdS QDs is ∼5.3 nm. The d-spacings of the clear crystalline structure are 0.335 nm, 0.205 nm, and 0.352 nm, that can be indexed to (111) and (220) of CdS (JCPDS no. 80-0019) and (101) of anatase TiO2, respectively. EDS mapping of the sample is shown in Fig. 3E and the corresponding line scan profile of EDX spectra is shown in the ESI (Fig. S9†). The distribution and counts of the Cd and S elements are very similar, but different from those of the Ti and O elements; this indicates that the CdS crystal is the only form in which Cd and S exist. Fig. 3F shows the UV-vis spectra of the original sample and the sensitized sample. The absorption range greatly enlarges from ∼380 nm to 570 nm. The tuned band gap indicates that CdS QDs are well bonded onto the TiO2 hybrid structure and provide a good electronic transmission channel. Fig. 3G shows the XRD patterns of the sample. A new peak at 2θ = 26.5° is observed and indexed to CdS, which is in accordance with the abovementioned HRTEM results.
Fig. 3 SEM images (A and B), TEM and HRTEM images (C and D), EDS mapping (E), UV-vis spectra (F), and XRD patterns (G) of the CdS-sensitized hybrid structure. |
Photocurrent is usually seen as one of the key parameters of PEC performance and reflects the transfer efficiency of photo-excited electrons. Fig. 4A presents the photocurrent density characteristics (J–V curves) and photoconversion efficiencies of the samples. The photocurrent density at 0 V vs. Ag/AgCl (JSC) and photoconversion efficiency (η) of the hybrid structure are 1.36 mA cm−2 and 0.81% (−0.51 V vs. Ag/AgCl), respectively, nearly 2.4 times higher than those of bare TWTs (0.57 mA cm−2 and 0.35% at −0.42 V vs. Ag/AgCl). Furthermore, JSC and η of 1.53 mA cm−2 and 1.14% (−0.69 V vs. Ag/AgCl), respectively, were attained for the CdS-sensitized TWTs. These results confirm that CdS QD sensitization is an effective method for enhancing the PEC performance of TWTs. The JSC and η of the CdS-sensitized hybrid structure are found to be 2.31 mA cm−2 and 1.94% (−0.65 V vs. Ag/AgCl), respectively, about 1.5 times those of the CdS-sensitized bare TWTs, and the hybrid structure can boost the JSC and η of bare TWTs by up to 400%. Moreover, the PEC performance of the electrodes at various wavelengths was measured by the IPCE test. As shown in Fig. 4B, the best IPCE of the CdS-sensitized hybrid structure electrode is around 25% across the absorption ranges, which is higher than those of other electrodes (14% for CdS-sensitized TWTs > 6% for hybrid structure > 2% for TWTs), indicating that electron–hole pairs are more efficiently separated in the CdS-sensitized hybrid structure electrode. IPCE results of the samples are in accordance with the corresponding absorption spectra as well as the corresponding photocurrent–voltage (J–V) curves. Stability, reproducibility, and repeatability of the samples can be represented by transient photocurrent (J–T) plots. We generated the J–T plots at 0 V vs. Ag/AgCl under chopped illumination. The J–T responses of the samples are shown in Fig. 4C; all the samples show relatively good reproducibility and stability when illumination is turned on and off. The observed dark current densities (light off) for all the samples are negligible. It is obvious that the effect of CdS is more prominent in the CdS-sensitized hybrid structure system as a result of the improved distribution of the CdS QDs and the effective separation of the photo-generated charges.
The superior PEC performance of the CdS-sensitized hybrid structure can be ascribed to the following reasons: as illustrated in Fig. 5, the TiO2 nano-polyhedrons grown on TWTs not only increase the specific surface area of the electrode but also improve light utilization owing to the exposed highly active {001} facets. It is also noteworthy that a higher specific surface area can increase the interface are as between the electrode and electrolyte, which can effectively reduce the recombination rate of photo-generated electron–hole pairs and thus enhance the photocurrent density. Moreover, the TiO2 nano-polyhedrons grown on TWTs with highly active {001} facets provide more effective area for the adsorption of CdS, thus increasing the generation of electron–hole pairs. Moreover, as the conduction band edge of CdS is higher than that of TiO2, a type-II band structure is formed between CdS and TiO2, facilitating the transfer of photo-generated electrons from CdS to TiO2. The photoexcited electrons then move from CdS to TiO2 nano-polyhedrons or move from CdS to TWTs and are gathered on the Ti substrate; this leads to a considerably reduced electron–hole recombination and enhanced photocurrent and efficiency.
Footnote |
† Electronic supplementary information (ESI) available: Fig. S1 TEM images of hybrid structure. Fig. S2 XPS spectrum of hybrid structure. Fig. S3 PEC performance of hybrid structure samples prepared under different TiF62− concentration: J–V curves (A), photoconversion efficiencies (B). Fig. S4 SEM images of bare TWTs (A and B), CdS sensitized bare TWTs (C and D). Fig. S5 line scan profile of EDX spectra of CdS sensitized hybrid structure. See DOI: 10.1039/c7ra05772e |
This journal is © The Royal Society of Chemistry 2017 |