Seyed Mohsen Sadeghzadeh*a,
Rahele Zhianiab and
Shokufe Emraniab
aDepartment of Chemistry, Faculty of Sciences, Neyshabur Branch, Islamic Azad University, Neyshabur, Iran. E-mail: seyedmohsen.sadeghzadeh@gmail.com
bYoung Researchers and Elite Club, Neyshabur Branch, Islamic Azad University, Neyshabur, Iran
First published on 23rd June 2017
In this study, vitamin B12 (VB12) modified with a (3-glycidyloxypropyl)trimethoxysilane (GMSI) moiety grafted onto KCC-1 (KCC-1/GMSI/VB12) was prepared for the first time. Its capability was evaluated for the carbonylative Suzuki–Miyaura crosscoupling reaction between carbon monoxide, 4-iodoanisole and phenylboronic acid, affording the desired products in high yield. Applying 1 mg of catalyst and 1 mmol of K2CO3 as base in 10 mL anisole and heating under reflux for 1 h are the best conditions for the reaction. The catalysts were very active in catalytic recycling experiments over ten catalytic cycles.
The ability of vitamin B12 to catalyse these thermodynamically challenging reactions has attracted the attention of synthetic chemists. Vitamin B12 is as an environmentally benign catalyst in organic reactions, which has eventually led to the discovery of new catalytic transformations. Vitamin B12 is as a catalyst which need costly and difficult separation of the catalyst from homogeneous reaction mixtures. For solving this problem, the use of heterogeneous vitamin B12 is important advantages in organic synthesis, such as operational simplicity, reusability, non-toxicity, environmental adaptability, and ease of isolation. The use of recyclable strong heterogeneous vitamin B12 in organic reactions are often considered to follow the principles of green chemistry, such as operational simplicity, reusability, non-toxicity, environmental adaptability, and ease of isolation. Recently, Vivek Polshettiwar reported the synthesis of new fibrous silica nanosphere (KCC-1) with high surface area, large open pore structure, and high thermal and hydrothermal stabilities.10 Therefore, most of its surface area is accessible, yielding unusually high activity in catalysis.11–25 The KCC-1 is extremely favorable in the design of the inorganic–organic hybrid sensing materials owing to the unique physical properties such as easily accessible of active sites, large open pore structure, excellent solvent dispersibility, favorable biocompatibility, high surface area, and superparamagnetism. Herein, we present a facile synthesis of KCC-1 based nanoparticles and was further functionalized by a vitamin B12 with (3-glycidyloxypropyl)trimethoxysilane (GMSI) linker that have been applied as novel nano catalyst for the carbonylative Suzuki–Miyaura crosscoupling reaction (Scheme 1).
The SEM images of the KCC-1/GMSI/VB1 NPs catalysts were shown in Fig. 1. As can be seen from the Fig. 1a, the KCC-1/GMSI/VB1 NPs had a consistent particle size range of 260–380 nm. SEM image shown in Fig. 1a further clarifies that the distance between the two fibers was about 10–15 nm. The recyclability test was stopped after ten runs. Comparison of SEM images of used catalyst (Fig. 1b) with those of the fresh catalyst (Fig. 1a) showed that the morphology and structure of KCC-1/GMSI/VB1 NPs remained intact after ten recoveries. Agglomeration of KCC-1/GMSI/VB1 NPs can not be seen.
Fig. 1 SEM image of the fresh KCC-1/GMSI/VB12 NPs (a), and SEM images of KCC-1/GMSI/VB12 NPs after ten reuses (b). |
FT-IR spectroscopy was employed to determine the surface modification of the synthesized catalyst (Fig. 2). The bands at 802, 1103 and 1630 cm−1 observed in the FT-IR spectra of both KCC-1 is related to the typical silanol group (Si–OH) stretching mode, Si–O–Si vibrations and the water absorbed on the solid surface, respectively (Fig. 2b). FTIR spectrum of cobalamin is shown as a reference. The spectrum of VB12 shows two major parts. The broad peak at about 3400 cm−1 is assigned to the O–H stretching of the hydroxyl groups attached to the surface.26 The second peak is in around of 1665 cm−1. The CO stretching vibration due to propionamide side chain of VB12 caused the appearance of this intense peak at 1670 cm−1 (Fig. 2a).27–29 Peak appeared at 3390 cm−1, 3120 cm−1, 2930 cm−1, and 1665 cm−1 are due to the stretching of the hydroxyl group (–OH), the C–H aromatic group, the C–H aliphatic group, and CO group in the KCC-1/GMSI/VB12 NPs (Fig. 2c). By comparing the three parts of Fig. 2, the formation of a new band at 751 cm−1 is evident. Although, this peak is situated in the fingerprint region of the IR spectrum, a new event is detected after the VB12 loading process, whereas no such peak is observed in the pristine VB12 and KCC-1 spectra. This phenomenon can be an evidence for the conjugation of VB12 molecules to KCC-1 NPs.
The TG analysis of KCC-1/GMSI/VB12 NPs was determined and shown in Fig. 3. A significant decrease in the weight percentage of the KCC-1/GMSI/VB12 NPs at about 130 °C is related to desorption of water molecules from the catalyst surface. This was evaluated to be 1–3% according to the TG analysis. In addition, the analysis showed two other decreasing peaks. First peak appears at temperature around 250–280 °C due to the decomposition of Co. This is followed by a second peak at 420–460 °C, corresponding to the loss of the organic spacer group. The major concern is related with a plausible presence of trace amounts of other active metal (like Pd, Cu, Fe, Ni, Cd, and Co) in any component of the reaction. To solve this problem it was necessary to carry out an ICP analysis of the reaction components. You can see in Table 1 that the concentration of Pd, Cu, Fe, Ni, Cd, and Co were very low that discard the slightest doubt.
Entry | Element | Weight percent (%) |
---|---|---|
1 | Pd | — |
2 | Cu | <0.01 |
3 | Fe | <0.01 |
4 | Ni | — |
5 | Cd | <0.01 |
6 | Co | — |
To optimize the reaction conditions, the carbonylative cross-coupling reaction of iodobenzene with phenyl boronic acid in the presence of KCC-1/GMSI/VB12 as a catalyst was chosen as a model system. The influence of various parameters such as solvent, base, and time (Table 2) were examined on the model reaction. The influence of solvents on the carbonylative Suzuki coupling reaction was investigated (Table 2, entries 1–15). According to the evaluated results of solvents, when polar protic solvents, such as methanol, isopropanol, ethanol, and water, were showed that any amount of the desired product was not formed. However, the yield of the cross-coupling product was relatively average in polar aprotic solvents, such as DMF, CH2Cl2, EtOAc, CHCl3, anisole, and DMSO. When the reaction was conducted in less polar solvents, such as anisole or toluene, good to high yields of carbonylative cross-coupling product were isolated, and anisole was found to be the best choice. However, the carbonylative cross-coupling product was obtained in low yield in polar solvents. In this study, it was found that conventional heating under anisole is more efficient than using organic solvents (Table 2, entries 8). It is well known that bases play a crucial role in coupling reactions; hence we attempted the reaction in the presence of various organic and inorganic bases (Table 2, entries 16–26). As a result, the most used base K2CO3 was the most efficient base to produce carbonylative cross-coupling product. Under the optimal conditions, the reaction progress for the shortest time necessary in the presence of 2 mg of KCC-1/GMSI/VB12 NP was monitored by GC, that excellent yields of carbonylative Suzuki coupling reaction can be achieved in 1 h (Table 2, entries 26).
Entry | Solvent | Base | Time (h) | Yieldb (%) |
---|---|---|---|---|
a Reaction conditions: iodobenzene (1 mmol), phenyl boronic acid (1.2 mmol), KCC-1/GMSI/VB12 NPs (1 mg), K2CO3 (3 mmol), solvent (10 mL), CO pressure = 3 MPa.b Isolated yields. | ||||
1 | EtOH | K2CO3 | 1.5 | — |
2 | H2O | K2CO3 | 1.5 | — |
3 | CH3CN | K2CO3 | 1.5 | 46 |
4 | DMF | K2CO3 | 1.5 | 59 |
5 | CH2Cl2 | K2CO3 | 1.5 | 38 |
6 | EtOAc | K2CO3 | 1.5 | 21 |
7 | THF | K2CO3 | 1.5 | 32 |
8 | Toluene | K2CO3 | 1.5 | 63 |
9 | n-Hexane | K2CO3 | 1.5 | — |
10 | CHCl3 | K2CO3 | 1.5 | 32 |
11 | DMSO | K2CO3 | 1.5 | 41 |
12 | MeOH | K2CO3 | 1.5 | — |
13 | Dioxane | K2CO3 | 1.5 | — |
14 | i-PrOH | K2CO3 | 1.5 | — |
15 | Anisole | K2CO3 | 1.5 | 96 |
16 | Solvent-free | K2CO3 | 1.5 | — |
17 | Anisole | — | 1.5 | — |
18 | Anisole | CsF | 1.5 | — |
19 | Anisole | Na2CO3 | 1.5 | 62 |
20 | Anisole | Et3N | 1.5 | — |
21 | Anisole | NaOAc | 1.5 | — |
22 | Anisole | KOH | 1.5 | 43 |
23 | Anisole | K3PO4 | 1.5 | 70 |
24 | Anisole | Cs2CO3 | 1.5 | 67 |
25 | Anisole | tBuOK | 1.5 | — |
26 | Anisole | K2CO3 | 1 | 96 |
27 | Anisole | K2CO3 | 0.5 | 90 |
We also study the decisive role of temperature in the synthesis of carbonylative Suzuki–Miyaura reaction in the presence of KCC-1/GMSI/VB12 NPs as a catalyst. The best temperature for this reaction heating under reflux do cause changes in the efficiency of the reaction, that showed the catalytic activity is susceptible to reaction temperature. The catalyst loading is another important factor in current reaction for the carbonylative cross-coupling reaction (Fig. 4). As shown in Fig. 4, the low yield of carbonylative Suzuki–Miyaura reaction was gained when model reaction was performed in the absence of a catalyst. When 0.2–0.8 mg of KCC-1/GMSI/VB12 NPs were elaborated on sample reaction, moderate yields of carbonylative Suzuki coupling reaction were obtained. The best result was achieved when the model reaction was carried out in the presence of 1 mg of KCC-1/GMSI/VB12 NPs. A rise in the catalyst amount showed no upgrading in the model reaction. In the absence of the catalyst no product was obtained. Effects of CO pressure in the presence of iodobenzene, phenyl boronic acid, and KCC-1/GMSI/VB12 NPs for 1 h was shown in Fig. 5. The catalyst mixture reaches an average of >96% of conversion at 1 MPa pressure. No apparent by-products were observed by GC in all the experiments and carbonylative Suzuki–Miyaura reaction was obtained cleanly in 96% yield.
With the optimized reaction conditions, we extended the scope of carbonylative Suzuki reaction to a variety of different aryl iodides with phenyl boronic acids. As shown in Table 3, various electron-donating and electron-withdrawing groups such as –CH3, –OCH3, –NH2, –COCH3, –NO2, –Br and –Cl on both aryl iodide and aryl boronic acid smoothly underwent carbonylative Suzuki coupling reaction giving desired products with appreciable yields. Iodobenzene reacted with phenyl boronic acid giving 96% yield of benzophenone (Table 3, entry 1). It is worth noting that aryl iodides containing electron-withdrawing groups, such as –Br, –Cl, –COCH3 and –NO2, were found to be the more active than aryl iodides containing electron-donating groups, such as –CH3, –OCH3 and –NH2.
For further investigation the efficiency of the catalyst, different control experiments were performed and the obtained information is shown in Table 4. Initially, a standard reaction was carried out using KCC-1 showed that any amount of the desired product was not formed after 1 h of reaction time (Table 4, entry 1). Also, when KCC-1/GMSI was used as the catalyst, a reaction was not observed (Table 4, entry 2). The GMSI could not give the satisfactory catalytic activity under mild reactions. We compared the results achieved in this work with elsewhere over many other similar catalysts. In contrast with the catalysts of VB12 as a homogeneous catalysis our catalyst requires similar condition for the carbonylative cross-coupling (Table 4, entries 3 and 5). Also, the activity and selectivity of nano-catalyst can be manipulated by tailoring chemical and physical properties like size, shape, composition and morphology. To assess the exact impact of the presence of KCC-1 in the catalyst, the KCC-1/GMSI/VB12 NPs compared with SiO2/GMSI/VB12 NPs. To check this, we looked at SiO2/GMSI/VB12 and KCC-1/GMSI/VB12 NPs, which have the same compositions and different structures. When SiO2/GMSI/VB12 was used as the catalyst, the yield of the desired product was fair to average, but the yield for KCC-1/GMSI/VB12 was good (Table 4, entries 3 and 4).
Entry | Catalyst | Catalyst loading | Yieldb (%) |
---|---|---|---|
a Reaction conditions: iodobenzene (1 mmol), phenyl boronic acid (1.2 mmol), K2CO3 (3 mmol), solvent (10 mL), CO pressure 1 MPa after 1 hour.b Isolated yield. | |||
1 | KCC-1 | 1 mg | — |
2 | KCC-1/GMSI | 1 mg | — |
3 | KCC-1/GMSI/VB12 | 1 mol% | 96 |
4 | SiO2/GMSI/VB12 | 1 mol% | 59 |
5 | VB12 | 1 mol% | 97 |
We compared the catalytic performance of our catalyst with catalysts reported for carbonylative Suzuki coupling reaction (Table 5). Table 5 clearly demonstrates that the most favourable terms are required for carbonylative Suzuki coupling reaction, using KCC-1/GMSI/VB12 NPs, while an appropriate, highly perfect, performance of the present catalyst is observed for the reaction.
Entry | Catalyst | Experimental conditions | Yield (%) | Ref. |
---|---|---|---|---|
a Reaction conditions: iodobenzene (1.0 mmol), phenylboronic acid (1.2 mmol), in different temperature, time, and pressure of CO. | ||||
1 | Pd/C | 100 °C, 8 h, 4 bar CO | 90 | 30 |
2 | P(DVB-NDIIL)-Pd | 120 °C, 12 h, 30 bar CO | 86 | 31 |
3 | Fe3O4@SiO2-2N-Pd | 80 °C, 8 h, 1 bar CO | 91 | 32 |
4 | PS-Pd-NHC | 100 °C, 10 h, 7 bar CO | 94 | 33 |
5 | HMMS-SH-Pd | 80 °C, 9 h, 1 bar CO | 94 | 34 |
6 | MCM-41-2N-Pd | 80 °C, 8 h, 1 bar CO | 91 | 35 |
7 | KCC-1/GMSI/VB12 | Reflux, 1 h, 1 bar CO | 96 | This work |
To obtain information about the heterogeneity or homogeneity of the catalytic reaction, hot filtration and mercury poisoning tests were carried out. At first, the relationship between the progress of reaction and time was maximum at the range of 3–6 h. Thus, we chose the point of 5 h for the following experiments. The catalyst was filtered out at above 100 °C after the reaction proceeded for 6 h and the yield of benzophenone was 74% determined by GC. The obtained filtrate with additional 1.0 mmol phenyl boronic acid was continually stirred under the reaction conditions. After 6 hours the conversion was determined to be 74%. The same approach was applied to mercury test. After the first stage, the yield of benzophenone was 72%. In the second stage, after mercury (0.3 mL) was added into the filtrate, the filtrate was stirred for another six hours under the reaction conditions. The yield of benzophenone remained to be 74%. These phenomena show that a small amount of catalytically active VB12 species may have leached to the reaction mixture (Fig. 6). But the contents of VB12 in catalyst before and after reaction were 5.7% and 5.5% respectively, determined by ICP-MS. These indicate that most of VB12 species leaching into solution are recaptured onto the fibers of KCC-1 after completion of the reaction (Table 6). It is important to note that the heterogeneous property of KCC-1/GMSI/VB12 NPs facilitates its efficient recovery from the reaction mixture after the completion of reaction. The amount of VB12 in KCC-1/GMSI/VB12 NPs were similar after reused for ten consecutive periods of catalysts. Notably, the catalyst could be recycled up to ten times with a marginal decrease in activity (Fig. 7).
Entry | Catalyst | wt% |
---|---|---|
1 | KCC-1/GMSI/VB12 NPs | 5.7 |
2 | KCC-1/GMSI/VB12 NPs after ten reuses | 5.5 |