Chi-Nan Chenga,
Rong-Ting Lioua,
Jenn-Ming Song*a and
Shao-Ju Shihb
aDepartment of Materials Science and Engineering, National Chung Hsing University, Taichung, Taiwan. E-mail: samsong@nchu.edu.tw
bDepartment of Materials Science and Engineering, National Taiwan University of Science and Technology, Taipei 106, Taiwan
First published on 22nd August 2017
Silver acetate instead of silver nitrate was used as the precursor to synthesize submicron-sized Ag particles (Ag SMPs) using a thermal-spray pyrolysis method at relatively low processing temperatures. Pastes comprised of Ag particles were produced and sintered at 100 °C or 250 °C to form conductive circuits for different-level microelectronics. The produced circuits were designed for application as interconnections in consumer and automotive devices. The critical current necessary to fuse the circuit was measured to evaluate the interconnect reliability under high-power electrical current stress. The experimental results show that a critical calcination temperature exists between 350 to 400 °C for full silver acetate conversion into Ag powders. The amount of residual precursor, morphology, constituent and size of the Ag particles, as well as the electrical conductance of the sintered structures are all influencing factors. When subjected to heating at 100 °C for 10 min, the sintered conductive Ag SMP lines can withstand current stress density exceeding 1 mA μm−2 under 12 V, indicating superior electrical reliability. The low-temperature sintered SMP deposits also demonstrated excellent bending fatigue resistance.
Ultrasonic spray pyrolysis (SP) has been developed to fabricate fine metallic powders because of its low cost, one-step continuous processing, high purity and chemistry flexibility.2,3 It is also recognized as an energy-efficient solution based method wherein high frequency ultrasound passes through a liquid precursor solution and forms an aerosol of micron-sized droplets, which are carried by gas flow into a heated zone where solvent evaporation and reactions occur.3 Table 1 tabulates previous studies about the spray pyrolysis of Ag particles.4–10 AgNO3 (silver nitrate), Ag2CO3, Ag2O and AgC2H3O2 (silver acetate) have been used as precursors. As indicated, calcination temperatures are set to range from 400 °C to 1000 °C according to the precursors, the solvents and the atmosphere. No data of the electrical conductance of sintered structure of the pyrolyzed Ag particles are available. In addition to solid particles with nanosizes or submicron-sizes,4–6,9,10 fine Ag particles with mesoporous7,8 or alloyed structure11–13 can also be synthesized using this method. Ag based composite particles with glasses or oxides have been applied in antibiotics and surface enhanced Raman scattering.14–16
Precursor | Calcination temperature without residual precursors (°C) | Atmosphere | Electrical resistance of sintered structure | Ref. | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
a NH4OH as the solvent. | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
AgNO3 | 600–1000 | N2 | N.A. | 4 | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
AgNO3 | 400–800 | N2 + H2 | N.A. | 5 | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
AgNO3 | 790 | Air | N.A. | 6 | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
AgNO3 | 700 | N2 | N.A. | 7 | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Ag2CO3 | 640 | Air | N.A. | 8 | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Ag2CO3 Ag2Oa | 400 | N2 | N.A. | 9 | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
AgC2H3O2 | 400–800 | Air | N.A. | 10 |
To prevent particle coarsening and oxidation at elevated temperatures, silver acetate, with a lower decomposition temperature has been recently chosen to replace the most commonly used precursor, silver nitrate.10 Fig. 1 shows concise data about the decomposition of two aforementioned silver salts, the dissociation of silver acetate starts from 200 °C to 265 °C, while that of silver nitrate is from 370 °C to 460 °C. However, the literature suggests that a calcination temperature of 600 °C and above is still needed for the complete decomposition of silver acetate in air.10 For the particles treated at 400 and 600 °C, a bimodal distribution (nanometer size and sub-micrometer size) could be found, while the particles treated at 800 °C exhibited a normal distribution (submicron size only).
Using silver acetate as the precursor, this study develops interconnect materials for different level packaging using thermal spray pyrolysis. In consideration for saving energy, the pyrolysis temperature was lowered to range from 250 °C to 500 °C. In order to prepare interconnections for polymeric substrate or repair PCB (printed circuit board) circuits, the particle sintering temperature was reduced to 100 °C. High power current stress and bending fatigue tests for the interconnection were carried out to evaluate the interconnection reliability.
The thus formed powders were characterized using TGA (thermogravimetric analysis), X-ray diffractometer, and FTIR (Fourier transform infrared spectroscopy). Ag pastes were prepared by mixing Ag particles and α-terpineol. Ethyl cellulose was added to thicken the pastes. Isothermal heat treatments of the pastes were performed at 100 °C for 10 min or 250 °C for 30 min to simulate different-level interconnect manufacturing processes. Commercial sinter pastes (α-metal Argomax2020) comprised of Ag nanoparticles with an average diameter of 20 nm were adopted for comparison.
The electrical properties of the sintered powders were measured using the four-point method. The current stress test was carried out using the pattern on Si chips sketched in Fig. 3, where the pastes were printed onto the dark gray area. Considering that laptops and automotive electronics run on 12 V electric current, a constant voltage of 12 V was conducted through the stripe connecting the two trapezoid pads, which had a length of 6 mm and width of 0.4 mm.
The fatigue performance of the sintered Ag films on the PET (polyethylene terephthalate) substrate was evaluated using the cyclic bending fatigue test. The cyclic bending test was carried out at a frequency of 2 Hz for 10000 cycles. The electrical resistivity corresponding to the bending cyclic number was recorded. The outer bending radius of the PET film (R) was 4.5 mm, which was obtained according to the following equations.17
![]() | ||
Fig. 4 Ag powders subjected to spray pyrolysis at different temperatures: (a) 250 °C, (b) 300 °C, (c) 350 °C, (d) 400 °C and (e) 500 °C. |
The FTIR results illustrated in Fig. 6 reveal that at 400 °C and above CO2− ligands at 1300–1700 cm−1 (ref. 18) completely diminished. Thermogravimetric analytic data reveal more information about the residual salts. Fig. 7 displays a decrease in weight for those calcined at 350 °C or below can be clearly seen upon heating. As shown in those curves, the reduction in weight stopped at about 250 °C. The residual AgC2H3O2 content for each condition can also be obtained from the TGA curves, i.e. 28.1 wt% for the powders calcined at 250 °C, 6.9 wt% for 300 °C and 2.3 wt% for 350 °C. For the powders calcined at 400 °C and 500 °C, the thermal-sprayed powder weight remained unchanged upon heating. The above results demonstrate that a critical pyrolysis temperature exists between 350 °C and 400 °C for the complete decomposition of silver acetate, which was much lower than the reported values in the literature except for those calcined in a reductive atmosphere.5,9 TGA measurement of the powders made from AgNO3 (AgN400) were also performed for comparison (Fig. 7). It can be found subjected to calcination at 400 °C, AgN400 shows a significant weight decrease upon heating, which can be ascribed a certain amount of undecomposed precursors.
![]() | ||
Fig. 8 Electrical resistivities of the sintered structures from Ag SMPs synthesized at different calcination temperatures (those using commercial nano-Ag pastes were given for comparison). |
Fig. 9 illustrates the sintered structures of the pastes comprised of AgA400 submicron particles and nano-Ag pastes subjected to heating at different temperatures. By comparison, it can be identified that the sintered structures of Ag submicron particles after heating at 100 °C for 10 min (Fig. 9(a)) or 250 °C for 30 min (Fig. 9(b)) did not differ too much. Both of them still revealed submicron grain size and necking at localized regions. In contrast, Ag nanoparticles coalesced at 100 °C (Fig. 9(c)) and grew further to micron-size while heated at 250 °C (Fig. 9(d)). It is remarkable that the sintered structure shown in Fig. 9(d) (nano-Ag heated at 250 °C) was much coarser than that in Fig. 9(b) (AgA400 heated at 250 °C). This can explain the drastic decrease in electrical resistivity of nano-Ag when the heating temperature was increased from 100 °C to 250 °C. It can be considered that 250 °C is enough for a more complete surfactant desorption for nano-Ag. The stacking of nano-sized particle deposits was much denser than that of submicron-sized particles; thereby the sintering and linking among the particles were more complete. The partially-sintered structure of AgA400, which was free of organic surfactants, still exhibited excellent electrical conductance.
With respect to the capability to endure high-power electrical current, Fig. 10 indicates that all the Ag SMP pastes subjected to heating at both 100 °C and 250 °C could withstand stress current density exceeding 1 mA μm−2 under a constant voltage of 12 V, except those with calcination temperature of 250 °C. The performance was at the same level of nano-Ag sintered conductive tracks cured at 250 °C. As for the lower critical current of 100 °C cured nano-Ag pastes (0.62 mA μm−2), the non-decomposed surfactants in the nanoparticles may account for that. Unlike the electrical or electromigration of nano-metal sintered structures studied in previous reports,19,20 the failure mechanism in this high-power electrical stress was melting of the Ag conductive lines.
![]() | ||
Fig. 10 Critical current density necessary to fuse interconnections prepared using thickened Ag pastes. |
The morphologies of the sintered deposits subjected to 10000 bending cycles are illustrated in Fig. 12. Both the sintered films were well attached on PET substrates without apparent peeling off or detachment. However, some strip-like loose regions can be found in the sintered nano-Ag, and no such regions were observed for sintered AgA400. This somehow explain the inferior electrical conductance of nano-Ag compared with AgA400 subjected to sintering at 100 °C. Undesorbed surfactants which were trapped in the sintered deposits (as shown in Fig. 9(c)) caused structural loosening and thus lower electrical conductance.
![]() | ||
Fig. 12 Surface morphologies of sintered films on PET subjected to 10![]() |
This journal is © The Royal Society of Chemistry 2017 |