Hierarchical porous metal–organic frameworks (HP-MOFs) with tunable porosity are highly valuable for many applications. Here, we developed a versatile solvothermal method to synthesize various HP-MOFs, such as Cu–BTC and ZIF-8, by using an organic amine as the template. The resulting HP-MOF products were characterized by a complementary combination of X-ray powder diffraction, Fourier-transform infrared spectroscopy, scanning electron microscopy, transmission electron microscopy, nitrogen adsorption–desorption isotherms, pore size distributions analysis, thermogravimetric analysis, and density functional theory calculations. The results indicated that the obtained HP-MOF products had high thermal stability and contained multimodal hierarchically porous structures with mesopores or macropores interconnected with micropores. In addition, the porosities of the produced HP-MOFs could be easily tuned by controlling the amount of the template. The introduced organic amine served as the template to direct the formation of mesopores and macropores. Furthermore, the synthesis route is highly versatile as other organic amines (e.g., N,N-dimethylhexadecylamine and N,N-dimethyltetradecylamine) can also be used as templates to synthesize HP-MOFs. The method developed in this work may offer a new direction to synthesize various stable HP-MOFs with tunable porosities for a wide range of applications.
To solve the diffusion and accessibility problems that guest species face in conventional MOFs with micropores, hierarchical porous MOF materials (HP-MOFs; MOFs with micro- and mesopores, or MOFs with micro-, meso-, and macropores) with tunable porosity, such as Cu–BTC,20 ZIF-8,21 and Zn–MOF-74,22 have been successfully synthesized since 2008. The extended pore structures (mesopores or macropores, or both mesopores and macropores) in HP-MOF materials can improve the diffusion rate and facilitate mass transfer of reactants or products. So far, four main methods have been developed to enlarge the pore size of conventional MOFs: ligand extension,23 post-processing,24 the use of mixed ligands,25 and templating.26 However, smaller mesopore size (<10 nm), volatility, instability, and vulnerable interpenetrating frameworks are almost unavoidable in HP-MOF products synthesized by the ligand-extension method.14 In addition, the post-processing and mixed-ligand methods tend to generate mesopores with uncontrollable size in the resulting HP-MOFs.27 For the template method, surfactants (ionic and neutral) or block copolymers are usually used as templates to direct the formation of mesopores in the internal MOF crystals.16 They can be easily manipulated and are feasible for preparing stable HP-MOFs with controllable porosity.14,28 For example, cetyltrimethylammonium bromide (CTAB) has been reported as a template that can be used to synthesize stable hierarchical porous Cu–BTC and ZIF-8.20,29 The triblock copolymers P123 and F127, which are widely applied to synthesize mesoporous zeolites, have also been used as templates to prepare stable HP-MOFs (e.g., Cu–BTC).30–32 Other new kinds of templates have also been reported for the synthesis of HP-MOFs, such as amphiphilic dodecanoic acid (DDA),33 N-ethyl perfluorooctylsulfonamide (N-EtOFSA),28 and 4-(dodecyloxy)benzoic acid (DBA).34 However, the species of templates reported to date that can be applied to synthesize HP-MOFs are limited. Therefore, it is highly desirable to extend the species of templates for the preparation of HP-MOFs with tunable porosity.
In this work, we adopted a new surfactant—organic amine—as the template and developed a solvothermal route to synthesize two stable HP-MOFs, Cu–BTC and ZIF-8. The porosity of the HP-MOF materials could be controlled by varying the molar concentration of the template. In addition, the molecular properties of the organic amine were studied based on density functional theory (DFT), with the amine group easily attacked by electrophilic species. Furthermore, a possible mechanism for the template synthesis of HP-MOFs was investigated. Other organic amines (e.g., N,N-dimethylhexadecylamine and N,N-dimethyltetradecylamine) could also be used as templates to synthesize hierarchical porous MOFs, demonstrating the versatility of our synthesis method.
The morphologies and porous structures of the as-synthesized MOF products were revealed by SEM and TEM. While the C-Cu–BTC particles had octahedral shapes with smooth surfaces (Fig. S2†), all of the as-synthesized Cu–BTC_An samples consisted of block-shaped particles with disordered pores of 20–100 nm in size between these particles (according to the pore size distribution (PSD, Fig. 3b)), as shown in the SEM images in Fig. 2a–c. The difference between the crystal morphology of C-Cu–BTC and Cu–BTC_An can be attributed to the effect of the introduced template.16,46,47 In addition, these Cu–BTC_An samples. Furthermore, it can be seen in Fig. 2a–c that all Cu–BTC_An samples exhibit smaller particle sizes (∼100 nm) than C-Cu–BTC (∼10 μm, Fig. S2†), which is in good agreement with the broader XRD peaks of Cu–BTC_An in Fig. 1a. As expected, high-resolution TEM offered insight into the local structure of the crystalline phases.48 As shown in Fig. 2d–f, these Cu–BTC_An samples also exhibit similar shapes and pore structures, with dense, uniform nanoflakes randomly stacked together and abundant voids in between. Cao et al.49 and Hirai et al.50 also reported that hierarchical porous structures in MOFs are formed through the aggregation or packing of microporous nanoparticles. Although void structures are clearly observed in all of the Cu–BTC_An samples (Fig. 2), their pore sizes differ depending on the amount of the template used.
Fig. 2 SEM and TEM images of the hierarchical porous Cu–BTC_An (n = 1, 2, 3) materials: (a, b) Cu–BTC_A1; (c, d) Cu–BTC_A2; (e, f) Cu–BTC_A3. |
The representative N2 adsorption–desorption isotherms and pore size distributions (PSDs) in Fig. 3 illustrate the porosity of the Cu–BTC_An samples. As shown in Fig. 3a, the isotherms of the three samples represent an intermediate mode between type I and type IV,26 in which the high uptake of adsorbates at the initial stage confirms the presence of micropores. The apparent hysteresis loop in the relative pressure range between 0.8 and 1.0 indicates the wide size distribution of mesopores,20,51 but these features do not appear in the isotherm of C-Cu–BTC. These analysis results confirm that micropores and mesopores were present in the Cu–BTC_An products, and similar conclusions were drawn from the works of Bradshaw et al.16 and Sun et al.,26 in which a series of hierarchical porous MOFs were synthesized by a template strategy, and the isotherms of the obtained MOFs showed a sharp increase in the uptake of adsorbates and an apparent hysteresis loop, revealing the formation of both micropores and mesopores. In addition, the isotherms of different Cu–BTC_An samples indicate obvious differences in their adsorption capacities, and the hysteresis loops that vary with the molar concentration of the template indicate the differences in the porosity of the samples.51 More detailed information regarding the porosity of Cu–BTC_An materials is acquired from the PSDs. As shown in Fig. 3b, in addition to the intrinsic micropores (0.8–0.9 nm in diameter), the as-synthesized Cu–BTC_An contains pores with a broad range of pore sizes from 20 to over 100 nm, including regions of meso- and macroporous regions that are absent in C-Cu–BTC. Although there have been a couple of reports of Cu–BTC with both micro- and mesopores,16,52 such hierarchical porous Cu–BTC material with pore diameters encompassing three ranges (micro-, meso-, and macropores) are, to the best of our knowledge, quite rare. Interestingly, the pore volume of Cu–BTC_An increases with increasing template concentration (inset of Fig. 4b), and similar trends can be seen in the summary of data in Table 1. These results not only validate the generation of mesoporosity in the Cu–BTC_An samples, but also indicate that the porosity of hierarchical porous MOFs could be controlled by the amount of template used during synthesis. In addition, the pore size distributions of H-MOFs exhibited consistency when the synthesis is repeated, as shown in Fig. S3.† Furthermore, we achieved the same porosity in the H-MOFs even for scaled-up syntheses using 2 and 10 times the original amounts of the materials, as shown in Fig. S4.†
Fig. 4 (a) Molecular electrostatic potential map (MEP); (b) surface of molecular orbital of N,N-dimethyloctadecylamine (legend of atoms: white = H; gray = C; blue = N). |
Samples | SBETa [m2 g−1] | Smicrob [m2 g−1] | Smeso/Smicroc | Vtd [cm3 g−1] | Vmesoe [cm3 g−1] | Dmesof [nm] |
---|---|---|---|---|---|---|
a SBET: Brunauer–Emmett–Teller (BET) surface area.b Smicro: micropore surface area calculated using the BET equation.c Smeso: mesopore surface area calculated using the BET equation.d Vt: total pore volume determined by using the adsorption branch of the N2 isotherm at P/P0 = 0.99.e Vmeso: mesopore volume based on the density functional theory (DFT) method.f Dmeso: mesopore diameter is determined from the local maximum of the BJH distribution of pore diameters obtained in the adsorption branch of the N2 isotherm. | ||||||
C-Cu–BTC | 1399 | 1313 | 0.08 | 0.60 | 0.05 | 1.8 |
Cu–BTC_A1 | 1231 | 1026 | 0.20 | 0.66 | 0.19 | 7.2 |
Cu–BTC_A2 | 1325 | 1074 | 0.23 | 0.79 | 0.29 | 11.9 |
Cu–BTC_A3 | 1351 | 1080 | 0.25 | 0.81 | 0.31 | 12.7 |
The porosity properties of the hierarchical porous Cu–BTC_An (n = 1, 2, 3) and C-Cu–BTC are summarized in Table 1. All of the Cu–BTC_An samples exhibit lower Brunauer–Emmett–Teller (BET) surface areas (SBET) than C-Cu–BTC, which can be attributed to the increased fraction of meso- and macropores decreasing SBET. Similar conclusions were drawn from the works of Qiu et al.,20 Yue et al.,22 and Huang et al.14 However, all Cu–BTC_An products have much higher total pore volumes (Vt) and mesopore volumes (Vmeso) than C-Cu–BTC, confirming the generation of mesopores in the Cu–BTC_An samples. In addition, as the amount of template is increased from 0.45 to 4.5 mmol during synthesis, Vt of the MOF products is increased from 0.66 (for Cu–BTC_A1) to 0.81 cm3 g−1 (for Cu–BTC_A3), and Vmeso is also increased from 0.19 to 0.31 cm3 g−1. Moreover, the mesopore diameter is increased from 7.2 to 12.7 nm as the amount of template is increased. Therefore, the porosity of the hierarchical porous MOFs was readily tuned by varying the amount of template added during synthesis.
Thermogravimetric analysis was performed under a N2 atmosphere to assess the thermal stability of the obtained hierarchical porous Cu–BTC_An. It can be seen from Fig. S5† that the initial stage of weight loss in all samples occurred at 100 °C owing to the evaporation of trapped solvent (e.g., deionized water).53,54 The second stage of weight loss in Cu–BTC_An was observed at approximately 220 °C, which probably corresponds to the loss of guest molecules in the pore channels.55,56 As shown in Fig. S5,† the weight of all samples dropped sharply after 300 °C, which can be attributed to the structural decomposition of Cu–BTC_An crystals.57 The TGA curves of Cu–BTC_An exhibited a consistent trend indicating that the amount of added template had no significant impact on the thermal stability of the hierarchical porous MOFs. In addition, the hierarchical porous MOF products exhibited weight change curves similar to that of C-Cu–BTC during the same thermal treatment, indicating that the as-synthesized hierarchical porous Cu–BTC_An had high thermal stability.
The organic amine molecules used in the present work contained amine groups and alkyl chain moiety, and the molecular electrostatic potential (MEP) of the template was calculated by using the DFT-B3LYP method and the 6-31G* basis set. The negative region (red) of the MEP is related to electrophilic reactivity, and the positive region (blue) to nucleophilic reactivity.58 As shown in Fig. 4a, the negative region of the N,N-dimethyloctadecylamine molecule is mainly concentrated on the amine group at the tail end, which represents the most susceptible sites for electrophilic attacks.59 Fig. 4b shows the distributions of the highest occupied molecular orbital (HOMO) calculated at the B3LYP/6-31G* level for the N,N-dimethyloctadecylamine molecule. The HOMO energy is directly related to the ionization potential and characterizes the susceptibility of a molecule toward attack by electrophiles.60 As shown in Fig. 4b, the HOMO is also mainly located in the amine group. The analysis confirms that the amine group of N,N-dimethyloctadecylamine is easily attacked by electrophilic species. Based on the above findings and results reported in the literature,16 a possible mechanism for the synthesis of hierarchical porous MOFs by using N,N-dimethyloctadecylamine as the template is illustrated in Scheme 1. In the initial stages, N,N-dimethyloctadecylamine formed supramolecular micelles through self-assembly,61,62 and then H contained in the ligands (H3BTC) interacted with the amine group of the template because the negative region was mainly concentrated in the tail-end amine group that easily attracted electrophilic species.60 When the Cu(NO3)2 solution was added, the Cu2+ and BTC3− ions began to self-assemble in the presence of the template. Finally, the template was removed to yield mesopores and/or macropores with walls formed by the crystalline microporous MOF.26 Qiu et al.,20 and Sun et al.,63 also reported a similar mechanism for synthesizing hierarchically structured MOFs by using a template strategy.
Based on the above synthesis mechanism, two other organic amines (N,N-dimethylhexadecylamine and N,N-dimethyltetradecylamine, Table S1†) were chosen as templates to synthesize hierarchically porous Cu–BTC, and the resulting products are named as Cu–BTC_B and Cu–BTC_C, respectively (see ESI†). As shown in Fig. S6,† the XRD pattern of the as-synthesized Cu–BTC_B powder matched well with that of C-Cu–BTC, indicating that the obtained product possessed the representative Cu–BTC framework. The isotherm of Cu–BTC_B showed an intermediate mode between type I and type IV, indicating the co-existence of micropores and mesopores (Fig. S7a†). The hierarchical porous structures with micro-, meso-, and macropores of Cu–BTC_B were further confirmed by the PSD, as shown in Fig. S7b.† The SEM and TEM images also exhibited obvious void structures in the Cu–BTC_B powder (Fig. S8†). In addition, Cu–BTC_C also exhibited a hierarchical porous structure (see Fig. S9–11 in ESI for additional data†). These results confirm that other organic amines could also be used for synthesizing HP-MOFs, demonstrating the versatility of the synthesis route.
Hierarchical porous ZIF-8 was also synthesized under hydrothermal synthesis conditions by using organic amine as the template (see ESI†). As shown in Fig. 5a, the XRD pattern of the as-synthesized hierarchical porous ZIF-8_A (the suffix A means that N,N-dimethyloctadecylamine was used as the template) agrees with that of conventional ZIF-8 (C-ZIF-8), indicating that the obtained product was crystalline ZIF-8. The FTIR spectrum of ZIF-8_A is in good agreement with that of C-ZIF-8, indicating that ZIF-8_A is phase-pure, as observed in Fig. 5b. The N2 adsorption–desorption isotherms of ZIF-8_A are a combination of type I and type IV isotherms with an apparent hysteresis loop (Fig. 6a), confirming the co-existence of micropores and mesopores in ZIF-8_A. Furthermore, the PSD of ZIF-8_A reveals that this product possesses mesopores and macropores (Fig. 6b). As shown in Fig. 6a, the hysteresis loop is absent from the isotherm of C-ZIF-8, which means that the conventional material did not contain mesopores and macropores. In addition, the SEM and TEM images (Fig. S12†) show obvious void structures in ZIF-8_A. Thermogravimetric analysis of the hierarchical porous ZIF-8_A and C-ZIF-8 reveals similar weight losses under the same thermal conditions (Fig. S13†), indicating that ZIF-8_A has good thermal stability.
Fig. 6 (a) N2 adsorption–desorption isotherms and (b) pore size distributions of ZIF-8_A and C-ZIF-8. |
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c7ra08798e |
‡ These authors contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2017 |