Guiqiang Wang*,
Shuo Hou,
Chao Yan and
Wei Zhang
School of New Energy, Bohai University, Jinzhou 121013, China. E-mail: wgqiang@bhu.edu.cn
First published on 3rd January 2018
A three-dimensional (3D) porous architecture combining porous vanadium nitride nanoribbons with reduced graphene oxide was prepared through a hydrothermal process and subsequent thermal annealing in an ammonia/argon mixed atmosphere. Then, the obtained 3D porous vanadium nitride nanoribbon/reduced graphene oxide (PVNN/RGO) composite was explored as the counter electrode of dye-sensitized solar cells (DSCs). As evidenced by the electrochemical measurements, the 3D PVNN/RGO composite demonstrates excellent electrocatalytic performance, which is comparable to that of Pt. This can be attributed to the fact that the 3D architecture composite of porous vanadium nitride and reduced graphene oxide can simultaneously provide a favorable electrolyte diffusion channel, a fast electron-transport network, and an abundance of efficient electrocatalytic active sites. By employing such PVNN/RGO composite as the counter electrode, the fabricated DSC can achieve a conversion efficiency of 7.43%, which is comparable to that of the conventional Pt counter electrode (7.74%). Therefore, the 3D PVNN/RGO composite is a promising low-cost alternative to the expensive Pt as a counter electrode in DSCs.
Recently, transition metal compounds, in particular, have gained attraction as counter electrode materials because of their low cost, ease of modification, and simple fabrication.16,27 Of the transition metal compounds investigated, transition metal nitrides display excellent electrocatalytic activity for reducing I3− to I− due to their noble metal-like surface electronic structure and the energy level.28–30 However, it is not easy for transition metal compounds to simultaneously display good electrical conductivity and superior electrocatalytic activity, even though it is an essential requirement for high-performance counter electrodes in DSCs. In general, nanoparticles can provide good electrocatalytic activity, but they increase the electron transport barrier owing to the abundant particle boundaries.
Constructing an efficient electron transport network and developing electrocatalytic active sites on the electron transport pathway is a promising strategy to synergistically combine electrical conductivity and electrocatalytic activity in a single material.31 Graphene and carbon nanotubes (CNT) can be considered as appropriate materials for creating a fast electron transport network. Cui et al. prepared transition metal nitrides/N-doped graphene hybrids, in which MoN, TiN, and VN nanoparticles were dispersed on the surface of N-doped graphene.32 These hybrid materials displayed higher photovoltaic performance than Pt. This improved performance is attributed to the combination of high electrical conductivity of the carbon electron-transport network and excellent electrocatalytic activity of transition metal nitride nanoparticles. Gao et al. prepared TiN–CNT composite by anchoring TiN nanoparticles on the CNT network,33 which showed a comparable photovoltaic performance with Pt.
Herein, a 3D architecture that combines porous vanadium nitride (VN) nanoribbons with reduced graphene oxide (RGO) was prepared and investigated as a counter electrode for dye-sensitized solar cells. The 3D architecture results in the formation of the interconnected hierarchical pore structure, which provides a favorable channel for electrolyte diffusion and then enhances the accessibility of electrode material. The highly conductive RGO network improves the electrical conductivity, and the porous nanoribbon structure of VN increases the electrochemically active surface area. As a result, the porous VN nanoribbon/reduced graphene oxide (PVNN/RGO) composite electrode displayed an excellent electrocatalytic activity for the reduction reaction of I3−. The DSC based on the PVNN/RGO counter electrode achieved a conversion efficiency of 7.43%, which is comparable to that of the cell based on a Pt counter electrode.
For the fabrication of TiO2 photoanodes, a TiO2 colloidal paste was prepared by mixing TiO2 (P25), Triton X-100, and hydroxypropyl cellulose in a mixed solution of deionized water and isopropanol with a volume ratio of 3:7. Then, the TiO2 electrodes were prepared by coating the TiO2 colloidal paste on FTO glass using the doctor-blade method and subsequent sintering at 450 °C for 30 min. The thickness of the TiO2 film was about 9 μm. Then, the as-prepared TiO2 electrodes were immersed in a 0.5 mM ethanol solution of N719 dye at room temperature for 16 h. Finally, the dye-sensitized TiO2 electrodes were rinsed with absolute ethanol. A DSC was fabricated by assembling a dye-sensitized TiO2 electrode, the electrolyte, and a counter electrode in a sandwich structure. The electrolyte was composed of 0.3 M LiI, 0.5 M 1-hexyl-3-methylimidazolium iodide, 0.05 M I2, and 0.4 M 4-tert-butylpyridine with 3-methoxyproponitrile as the solvent.
Fig. 2 (a, b) SEM images of the as-prepared 3D PVNN/RGO composite, (c) energy dispersive X-ray spectrum and elemental mapping for a rectangular area indicated in (a). |
The Brunauer–Emmet–Teller (BET) surface area and the pore structure of the as-prepared 3D PVNN/RGO composite were determined by N2 adsorption measurement at 77 K. Fig. 3 displays the N2 adsorption–desorption isotherm and the pore-size distribution curve of the PVNN/RGO sample, which clearly suggest that the as-prepared PVNN/RGO composite possesses a hierarchical porous structure consisting of small mesopores (2–10 nm) and large mesoporous (10–50 nm). The BET surface area of the PVNN/RGO composite calculated from the desorption branch of the isotherms is 200.5 m2 g−1, which is higher than that of the pure VN sample (Fig. S3†). High surface area and the hierarchical porosity can increase the effective electrode/electrolyte interface and enhance the electrolyte diffusion within the electrode material, which are favorable characteristics for improving the electrochemical performance of the electrode material.
Fig. 3 N2 adsorption–desorption isotherms (a) and pore-size distribution curve (b) of the 3D PVNN/RGO composite. |
Fig. 4a shows the XRD curve of the as-prepared 3D PVNN/RGO composite. A broad peak at 2θ value of around 26° can be assigned to graphene stacking. Four strong diffraction peaks at 2θ values of 38.08°, 44.18°, 64.18°, and 77.06° are ascribed to the crystal planes of (111), (200), (220), and (311) of cubic VN (JCPDS card no. 73-0528), respectively. This indicates that vanadium oxide obtained by thermal decomposition of NH4VO3 transformed into VN. Raman spectroscopy was employed to further investigate the structural information of the 3D PVNN/RGO composite. Fig. 4b shows the Raman spectrum of the as-prepared 3D PVNN/RGO composite. The two peaks observed at around 1351 and 1589 cm−1 correspond to the characteristic D and G bands of graphene, respectively. The peaks at 283, 408, 490, 526, 691, and 991 cm−1 can be attributed to the typical modes of vanadium oxide, indicating that a tiny amount of vanadium oxide was formed on the surface of VN nanoribbons. Although the formed vanadium oxide layer was too small to be detected by XRD (see Fig. 4a), the vanadium oxide layer on VN surface exhibits a very well resolved Raman signature, which dominates the Raman spectrum due to the very low intensity of VN peaks.35
The PVNN/RGO composite was deposited on a pre-cleaned FTO glass substrate by a spraying method. Electrocatalytic activity of the PVNN/RGO electrode for the reduction of I3− was investigated by EIS measurements using symmetric cells consisting of two identical electrodes. Fig. 5a shows the Nyquist plot of the PVNN/RGO electrode. For comparison, Nyquist plots of pure VN, RGO, and conventional Pt electrodes are also shown in Fig. 5a. As shown in Fig. 5a, Nyquist plots exhibit two semicircles, which are attributed to the Nernst diffusion impedance of the I−/I3− redox couple within the electrolyte and the charge-transfer process at the electrode/electrolyte interface in the order of increasing frequency. The inset in Fig. 5a is the equivalent circuit for the impedance spectra, where Rs is the serial ohmic resistance, Rct is the charge-transfer resistance, CPE is the constant phase element, and ZN is the Nernst diffusion impedance. EIS parameters (listed in Table 1) were determined by fitting Nyquist plots with Zview software. The Rs values of all the electrodes are primarily dominated by the resistance of FTO substrate. Therefore, the Rs of pure VN, RGO, and PVNN/RGO electrodes are comparable to that of the Pt electrode. The CPE of the PVNN/RGO electrode is noticeably higher than that of the pure VN electrode, indicating a higher active surface area of PVNN/RGO compared to pure VN. The Rct is a vital and widely used parameter to evaluate the electrocatalytic activity of the counter electrode for the reduction of I3−. As listed Table 1, the Rct values of Pt, PVNN/RGO, pure VN, and RGO electrodes are 1.02, 1.62, 8.12, and 15.21 Ω cm2, respectively. Clearly, the electrocatalytic activity of the PVNN/RGO electrode is higher than that of pure VN and RGO electrodes in the I−/I3− electrolyte. The enhanced electrocatalytic performance of the PVNN/RGO electrode can be attributed to its unique 3D porous architecture resulting from the combination of porous VN nanoribbons with RGO nanosheets. The 3D porous architecture can provide an interconnected channel for the fast diffusion of the electrolyte. Highly conductive RGO network is favorable for electron transport, and porous VN nanoribbons provide a higher effective surface area. The combination of these favorable features can greatly enhance the electrocatalytic performance of the PVNN/RGO electrode.
Fig. 5 (a) Nyquist plots of the cells fabricated with pure VN, RGO, PVNN/RGO, and Pt electrodes, (b) Tafel curves of pure VN, PVNN/RGO, and Pt electrodes. |
Electrode | Rs (Ω cm2) | Rct (Ω cm2) | CPE (μF) | Voc (V) | Jsc (mA cm−2) | FF | η (%) |
---|---|---|---|---|---|---|---|
Pt | 15.95 | 1.02 | 7 | 0.71 ± 0.01 | 16.52 ± 0.22 | 0.66 ± 0.01 | 7.74 ± 0.30 |
Pure VN | 16.17 | 8.12 | 65 | 0.69 ± 0.01 | 15.66 ± 0.21 | 0.58 ± 0.02 | 6.27 ± 0.39 |
PVNN/RGO | 16.18 | 1.62 | 326 | 0.71 ± 0.01 | 16.09 ± 0.25 | 0.65 ± 0.01 | 7.43 ± 0.33 |
RGO | 16.31 | 15.21 | 32 | 0.64 ± 0.02 | 13.59 ± 0.25 | 0.38 ± 0.02 | 3.32 ± 0.34 |
Tafel polarization measurements were conducted to further assess the electrocatalytic activity of the PVNN/RGO electrode. Fig. 5b displays the Tafel curves of dummy cells fabricated with pure VN, PVNN/RGO, and Pt electrodes. Tafel curve can be divided into three regions: the polarization zone, the Tafel zone, and the diffusion zone. In the Tafel zone, the exchange current density can be determined, which is directly related to the electrocatalytic activity of the electrode. Fig. 5b exhibits that the slope of the cathodic branch for the PVNN/RGO electrode is larger than that for pure VN electrode and comparable to that of the Pt electrode, indicating a higher exchange current density on the surface of the PVNN/RGO electrode. This result demonstrates that the PVNN/RGO electrode can catalyze the I3− reduction as effectively as the Pt electrode, which is in good agreement with the EIS result.
The photovoltaic performances of DSCs fabricated by PVNN/RGO, pure VN, RGO and Pt counter electrodes were obtained under an illumination of 100 mW cm−2. The current density–voltage curves are depicted in Fig. 6. The photovoltaic parameters of DSCs derived from Fig. 6 are summarized in Table 1. The RGO counter electrode exhibits a low conversion efficiency of 3.32% due to its poor electrocatalytic activity. The open-circuit voltage (Voc), the short-circuit current density (Jsc), the fill factor (FF), and the conversion efficiency (η) of the DSC assembled with the PVNN/RGO counter electrode are 16.09 mA cm−2, 0.71 V, 0.65, and 7.43% respectively. When pure VN was used as the counter electrode, the fabricated DSC showed a lower η of 6.27%, primarily due to a lower FF of 0.58. As we know, the FF is strongly influenced by the internal resistance of the DSCs. For DSCs fabricated with different counter electrodes, the Rct value of the counter electrode has a great effect on the FF of DSCs. As shown in Table 1, the Rct value of the PVNN/RGO electrode is measured to be lower than that of the pure VN electrode. Therefore, the PVNN/RGO counter electrode-based DSC has a higher FF. The photovoltaic parameters of the DSC with the Pt counter electrode are Voc = 0.71 V, Jsc = 16.52 mA cm−2, FF = 0.66, and η = 7.74%. Clearly, the photovoltaic performance of the DSC with the PVNN/RGO counter electrode is comparable to that of the DSC with the Pt counter electrode.
Fig. 6 Photocurrent density–voltage curves of DSCs with different counter electrodes measured at AM 1.5G illumination (100 mW cm−2). |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c7ra11279c |
This journal is © The Royal Society of Chemistry 2018 |