Ruiqi Naa,
Jinying Liub,
Guibin Wanga and
Shuling Zhang*a
aNational & Local Joint Engineering Laboratory for Synthesis Technology of High Performance Polymer, College of Chemistry, Jilin University, Changchun, 130012, P. R. China. E-mail: zsl@jlu.edu.cn; Fax: +86 431 85168868; Tel: +86 431 85168868
bChangchun Applied Chemistry Corporation Chinese Academy of Sciences, Changchun, 130012, P. R. China
First published on 16th January 2018
This study proposes an efficient method for fabricating a light weight and flexible composite film with excellent thermal stability and mechanical properties for wide-band electromagnetic interference (EMI) shielding, which was prepared by melt blending and subsequent melt extrusion using poly(ether ether ketone) (PEEK) as a matrix, multi-walled carbon nanotube wrapped poly(ether sulfone) (wrapped MWCNTs) as a conductive filler, and GENIOPLAST® PELLET S (GPPS, high-temperature lubricant) as a processing aid. GPPS was firstly used in EMI application, to reduce the melt viscosity of PEEK as well as to improve the dispersion of wrapped MWCNTs, which enables it to fabricate a highly efficient EMI shielding (∼74.6 dB mm−1) PEEK/wrapped MWCNT/GPPS1.0 composite film with a thickness of 180 μm. Furthermore, the lightweight composite film exhibits high thermal stability (i.e. degradation temperature at 5% mass loss of 586 °C) and good mechanical properties (tensile strength of 101 MPa), being superior to other previously reported EMI shielding films. The above mentioned enhanced property demonstrated its potential application as a high performance EMI shield for certain applications such as in the aerospace, weapons, and microelectronics industries, which require materials exhibits EMI shielding as well as superior mechanical properties and thermal stability.
Compared to conventional metal based EMI shielding materials, polymer composites containing carbon-based conductive fillers exhibit the advantages of being lightweight, flexible, corrosion-resistant, and easily processable.11,12 Specifically, multi-walled carbon nanotubes (MWCNTs) are excellent fillers for EMI shielding materials owing to their unique electrical, mechanical, and thermal properties.13–15 However, certain applications (e.g., aerospace, weapons, vehicles, and microelectronics) requiring materials with superior mechanical properties and thermal stability necessitate the use of high-performance polymers instead of general ones. Poly(ether ether ketone) (PEEK) is a semi-crystalline thermoplastic, high performance engineering polymer with superior mechanical properties, thermal stability, and corrosion resistance, being frequently used in the aerospace industry and electronics.16–20 More importantly, PEEK/MWCNT composite films can meet the requirements imposed on next-generation EMI shielding materials even in harsh environment.
The fact that MWCNTs are prone to agglomeration and are difficult to disperse in PEEK complicates, which restrict their use in EMI shielding materials.21 To solve this problem, we used MWCNTs wrapped in poly(ether sulfone) (noted as wrapped MWCNT) as a filler and a high-melt-index/low-melt-viscosity PEEK as matrix in our previous study, owing to the interaction between π-bonded surface of MWCNTs and the aromatic structure of the PES, the PES firm coating on the MWCNTs, which effectively avoiding the MWCNT agglomeration; secondly, the molecular structure of PES is similar to that of PEEK, which further enhancing their dispersibility in PEEK matrix.13,16 However, low-melt-viscosity PEEK is not suitable to produce flexible and thin composite films, using high-melt-viscosity PEEK as film matrix is necessary and still a challenge, since the low melt index and high melt viscosity properties of the high-melt-viscosity PEEK severely lead to failure of the filler dispersion and film processing. Besides, the EMI shielding effectiveness (EMI SE) of materials has mostly been evaluated in a narrow frequency range (8–12 GHz, X band),22–25 necessitating the development of advanced materials with good EMI SE in a wider frequency range of 8–40 GHz, which covers the bands used by civil, commercial, and military applications.20
In the present study, a series of PEEK/wrapped MWCNT/GENIOPLAST® PELLET S (GPPS) composite films with high flexible, good thermal and mechanical properties were prepared and applied to EMI shielding materials for the first time. PES was chosen as a coating for MWCNTs to ensure their strong interfacial adhesion and good dispersibility in PEEK matrix. Besides, we used a high-temperature lubricant, GPPS, in PEEK/wrapped MWCNT composites, which is an important silicone-based processing additive used in thermoplastics compounding in the plastics industry, for decreasing the melt viscosity of composites. In this system, the GPPS effectively reduce the melt viscosity of PEEK and further improve the dispersion of wrapped MWCNTs therein, to make it possible for the preparation of light weight and flexible PEEK/wrapped MWCNT/GPPS composite films, and improves the EMI SE in a wider frequency range of 8–40 GHz at the same time. The EMI SE, electrical conductivity, mechanical properties, and thermal stability of PEEK/wrapped MWCNT/GPPS composite films were discussed detailed in this study.
PEEK/MWCNT composites without and with GPPS were prepared by using a Mini-Haake co-rotating twin-screw extruder (Thermo Fisher Scientific, Waltham, Massachusetts, USA) at a screw speed of 40 rpm and a temperature of 390 °C. The obtained samples were noted as PEEK/MWCNT composite-GPPSx, where x is weight percent of the GPPS in the total PEEK and MWCNTs. The composites were cut into granules, then dried at 100 °C for 6 h in a vacuum oven, and then molded with the HAAKE MiniJet at a temperature of 400 °C and a pressure of 82 MPa for different measurements.
The above mixture was melt-blended (Haake PTW16/25p co-rotating twin-screw extruder, screw speed = 80 rpm, temperature profile = 270/350/355/360/365/360 °C) and granulated, with the obtained granules subsequently dried at 100 °C for 4 h.
Next, PEEK/wrapped MWCNT/GPPS composite films were fabricated by melt extrusion of dried granules using an arcuate-slit-head extruder at a screw speed of 120 rpm, a temperature profile of 270/350/360/365/370/380 °C, and a three-roller calender stretching speed of 2 m min−1.
It should be noted that the above molding process generally becomes very difficult at MWCNTs contents above 9 wt%, the composite films become discontinuous or uneven due to the increased filler content. Hence, the loading of wrapped MWCNTs did not exceed 9 wt% in this study.
Electrical conductivity measurements were performed at room temperature in a frequency range of 102–106 Hz using an Agilent 4294A precision impedance analyzer. The composites and films were cut into round specimens with a diameter of 10 mm, and two opposite surfaces of specimens were coated with silver conductive glue to ensure their good contact with electrodes.
The EMI SE of produced films was calculated based on vector scattering parameters S11 (as a measure of the forward reflection coefficient) and S21 (as a measure of the forward transmission coefficient), which were measured using an N5244A PNA vector network analyzer (Agilent, USA). For EMI shielding test, all film samples were cut into rectangular shapes, the film had a thickness of ∼180 μm, and the precisely dimensions at different frequency band are shown in Table S1.†
The densities (g cm−3) of composite film were measured by buoyancy method, using an electronic densimeter (SD-200L), from Alfa Mirage Co., Ltd, Japan. The composite films were cut into square shapes with a size of 20 mm × 20 mm × 0.18 mm, and each film sample was tested three times.
Tensile testing was conducted on a Shimadzu AG-1 universal testing machine at room temperature and a rate of 5 mm min−1, and tensile strength and elongation at break were also obtained from stress–strain curves. The gauge length, width and thickness of the test samples were 18.00 mm × 4.00 mm × 2.00 mm (length × width × thickness, for composites) and 18.00 mm × 4.00 mm × 0.18 mm (length × width × thickness, for composite films), respectively. The results of each composition were reported as average of at least three samples tests.
Thermogravimetric analysis (TGA) of composites and films were performed in air atmosphere, using a Perkin Elmer Pryis 1 TGA analyzer. For each measurement, 6 ± 1 mg of sample was heated at a heating rate of 10 °C min−1.
Fig. 1 (a) Dependence of AC conductivity of PEEK/MWCNT composite-GPPSx on frequency at room temperature. (b) Dependence of shear viscosity of PEEK/MWCNT composite-GPPSx on shear rate at 400°. |
The changes in the conductivity of the PEEK/MWCNT composite-GPPS depend on the dual roles of GPPS. On the one hand, the dispersion of the MWCNTs in the PEEK matrix could be improved as the content of GPPS in the composite increased, thereby increasing the conductivity of the composite. On the other hand, the content of MWCNTs dispersed in the PEEK matrix was reduced as the content of GPPS increased, due to the intrinsic insulativity of the GPPS, thus the conductivity of the PEEK/MWCNT composite-GPPSx decreased. A balance between these two effects is achieved with the optimal loading of GPPS of 1.0 wt%, which suggests that a small amount of GPPS (1.0 wt%) was sufficient to enhance the conductivity of the PEEK/MWCNT composites. Furthermore, the conductivity of the composites became independent of frequency in the range of 102–106 Hz. This may be because the content of MWCNTs was sufficient to effectively provide a tunnel for hopping of the electrons.
The high melt viscosity of PEEK with the low melt index generally lead to failure of the filler dispersion and processing; this disadvantage severely limits the applicability of this material. High-temperature lubricant GPPS is an important processing agent in decreasing the melt viscosity of composites. On the one hand, it can reduce the entanglement between the polymer chains, which helps to decrease the melt viscosity and achieve the better dispersion of filler in polymer matrix; on the other hand, it can decrease the friction between the composites and processing equipment which contributes to the improvement in the processability of flexible and thin composite films. Fig. 1b shows the shear viscosity of the PEEK/MWCNT composite-GPPSx without and with GPPS versus the shear rate, and the afore-mentioned phenomenon is substantiated by the data in this figure. The addition of GPPS evidently reduces the melt viscosity of the PEEK/MWCNT composite-GPPSx. Moreover, the shear viscosity of the PEEK/MWCNT composite-GPPSx composite gradually decreased with increasing GPPS content. Therefore, the addition of GPPS helps to decrease the melt viscosity in the processing temperature range of the PEEK/MWCNT composite, leading to better dispersion of the MWCNTs in the PEEK matrix and higher electrical conductivity of the PEEK/MWCNT composite.
To further illustrate the effect of the GPPS on the conductivity and melt viscosity of the PEEK/MWCNT composite, the detailed observation of the cross-section morphology of the PEEK/MWCNT composite and PEEK/MWCNT composite-GPPS1.0 were carried out and shown in Fig. 2. The dispersion of the MWCNTs in the PEEK/MWCNT composite without GPPS was relatively inhomogeneous (Fig. 2a), and the place without MWCNTs has been marked in the figure. In contrast, the MWCNTs are found to be homogenously dispersed in the PEEK/MWCNT composite-GPPS1.0 matrix (Fig. 2b), and almost no obvious aggregation of the MWCNTs was observed due to the regulation of the viscosity of GPPS. That is, the decrease in the melt viscosity of the PEEK matrix facilitates dispersion of the MWCNTs, thus improves the conductivity of the composites. This is in accordance with the changes in the conductivity and melt viscosity of the PEEK/MWCNT composite-GPPS without and with GPPS.
Fig. 2 SEM image of cross-section surface of (a) PEEK/MWCNT composite and (b) PEEK/MWCNT composite-GPPS1.0 (scale bar = 3 μm). |
The effect of GPPS on the mechanical properties of the PEEK/MWCNT composite were evaluated based on analysis of the tensile strength and elongation at break of the composites. The mechanical properties of the PEEK/MWCNT composite-GPPSx are summarized in Table 1. Generally, any aggregation of the MWCNTs could result in structural defects with detrimental effects on the mechanical properties.26 From Table 1, it could be found that the tensile strength of the composites remained almost unchanged (115 MPa) with increase of the content of GPPS from 0 to 1.0 wt%. However, with a further increase of the content of GPPS to 2.5 wt% and 5.0 wt%, the tensile strength decreased to 112 MPa and 108 MPa, respectively. In addition, the elongation at break initially increased and then decreased, when the content of GPPS increased from 0.0 wt% to 0.7 wt%, the elongation at break of the composites increased from 37.2% to 46.4%. However, the elongation at break gradually decreased from 45.1% to 35.1% with the amount of GPPS increased from 1.0 wt% to 5.0 wt%.
Amount of GPPS (wt%) | Tensile strength (MPa) | Elongation at break (%) |
---|---|---|
0 | 115 | 37.2 |
0.4 | 115 | 38.8 |
0.7 | 115 | 46.4 |
1.0 | 115 | 45.1 |
2.5 | 112 | 37.7 |
5.0 | 108 | 35.1 |
The changes in the mechanical properties of the PEEK/MWCNT composites depend on the dual roles of GPPS. On the one hand, the dispersion of the MWCNTs in the PEEK matrix were improved as the content of GPPS increases, i.e., the stress concentration of the PEEK/MWCNT composites was reduced during the tensile test, thereby increasing the tensile strength and elongation at break of the PEEK/MWCNT composites. On the other hand, the lower strength and toughness of GPPS as a processing aid becomes dominant with increasing content of GPPS higher than 1.0 wt%, thus the tensile strength and elongation at break of the PEEK/MWCNT composites decreases. Based on these two effects, it can be indicated that only a suitable amount of GPPS (1.0 wt%) was sufficient to enhance the electrical conductivity and mechanical properties of the PEEK/MWCNT composites.
The effect of adding GPPS to the composite on the thermal stability of the PEEK/MWCNT composite-GPPSx were evaluated via TGA under air atmosphere. Fig. 3 shows the thermal degradation curves of the PEEK/MWCNT composite and PEEK/MWCNT composite-GPPS1.0. The addition of GPPS did not impact the thermal stability of the PEEK/MWCNT composite. The temperature of 5% weight loss (Td5%) of the PEEK/MWCNT composite-GPPS1.0 is about 595 °C, which is almost equal to that of the PEEK/MWCNT composite. This phenomenon proves that the addition of GPPS did not produce a negative effect on the thermal stability of the PEEK/MWCNT composites, this can be ascribed to restriction of the thermal motion of the PEEK chains due to the better dispersion of the MWCNTs, thereby leading to higher thermal stability of the composites. The TGA curves of PEEK/MWCNT composite-GPPSx with different GPPS contents are given in Fig. S1.†
The above mentioned experimental data show that the addition of 1.0 wt% GPPS could effectively improve the electrical and mechanical properties of PEEK/MWCNT composite and not affecting its thermal stability, thus, the 1.0 wt% GPPS was chosen as the optimism constituent for further intensively studied.
In our previous study, we designed a EMI SE material, using poly(ether sulfone) (PES) wrapped MWCNTs (noted as wrapped MWCNTs) as conductive filler and dispersed in a high-melt-index/low-melt-viscosity PEEK matrix by melt-blending method, the MWCNTs wrapped in PES efficiently minimizing the agglomeration of MWCNT and enhancing their dispersibility, unfortunately, high-melt-index/low-melt-viscosity PEEK matrix used was not suitable for producing polymer films.13 In this study, a low-melt-index/high-melt-viscosity PEEK matrix was adopted to meet requirements of preparation PEEK-based composite films. However, high-melt-viscosity is not conducive to, even more harmful to the dispersion of MWCNTs for PEEK. In order to improve the dispersibility of MWCNTs in the high-melt-viscosity PEEK matrix, MWCNTs were modified by PES as well as addition of 1.0 wt% GPPS. We compared the conductivities and thermal properties of the PEEK/wrapped MWCNT/GPPS1.0 composite film with PEEK/MWCNT/GPPS1.0 composite film (both two kinds of composite films contain 1 wt% GPPS, and the weight ratio of the wrapped MWCNT or MWCNT are 7 wt%), the comparison results are shown in Fig. S2.† From Fig. S2,† it could be seen that the usage of PES wrapped MWCNTs can significantly enhance the conductivity of PEEK/MWCNT/GPPS1.0 composite film, which should be ascribed that the modification of PES on MWCNTs can avoid MWCNTs agglomeration and improve the dispersion of MWCNTs in PEEK. Additionally, the introduction of PES slightly decrease the thermal stability of PEEK/wrapped MWCNT/GPPS1.0 composite film, but its Td5% is still up to 583 °C, namely PEEK/wrapped MWCNT/GPPS1.0 composite film also possesses good thermal stability. Thus, to prepare composite film with high shielding effectiveness as well as enough thermal stability and mechanical properties, we choose wrapped MWCNTs as conductive filler, and 1.0 wt% GPPS as a processing aid, doing further investigation.
Fig. 4a shows room-temperature AC conductivities of PEEK/wrapped MWCNT/GPPS1.0 composite films as functions of frequency, with different PEEK/wrapped MWCNT proportion (PEEK wt%/wrapped MWCNT wt% = 100/0–91/9). The conductivities of composite films were significantly improved with increasing filler loading, and attained 1.29 S m−1 when the wrapped MWCNT up to 9 wt%. In addition, the conductivity of PEEK films increased with increasing frequency, implying insulating behavior. However, 1 wt% composite film showed a plateau followed by a gradual conductivity increase with increasing frequency, indicative of semiconducting behavior. At MWCNT loadings above 3 wt%, the conductivities of composite films became independent of frequency in the range of 102–106 Hz, which was mainly attributed to the fact that a certain content of wrapped MWCNTs was sufficient for them to interconnect and form conductive networks in the insulating PEEK matrix.
Fig. 4 (a) Electrical conductivities on frequency and (b) TGA curves of PEEK/wrapped MWCNT/GPPS1.0 composite films with different PEEK/wrapped MWCNT proportion. |
Thermal stability is an important parameter affecting the operational life of EMI shielding materials. Therefore, we investigated the thermal stabilities of the above mentioned PEEK/wrapped MWCNT/GPPS1.0 composite films by TGA test in air atmosphere. Fig. 4b illustrates the TGA curves of composite films with different wrapped MWCNT contents. The initial decomposition curves of composite films were shifted to higher temperature with the addition of MWCNTs, implying the increased thermal stabilities of the composite films. This phenomenon was rationalized as follows, on the one hand, MWCNTs possess good thermal stability,27 with their decomposition temperature of greater than 600 °C, exceeding that of pure PEEK; on the other hand, the network structure formed by MWCNTs in the PEEK matrix hinders the thermal motion of PEEK chains, thereby enhancing the thermal stability of PEEK. The 5% weight loss temperature (T5%) of composite films with 9 wt% wrapped MWCNT exceeded 586 °C, indicating their superior thermal stability.
Since the good mechanical properties and light-weight are important indicators determining the practical application of the films, the tensile strength, elongation at break and density of PEEK/wrapped MWCNT/GPPS1.0 composite films were evaluated and illustrated in Table 2.
PEEK/wrapped MWCNT (wt%/wt%) | Tensile strength (MPa) | Elongation at break (%) | Density (g cm−3) |
---|---|---|---|
100/0 | 89 | 180 | 1.2776 |
99/1 | 110 | 156 | 1.2932 |
97/3 | 109 | 128 | 1.3028 |
95/5 | 105 | 80 | 1.3150 |
93/7 | 102 | 62 | 1.3247 |
91/9 | 101 | 53 | 1.3380 |
The tensile strength of composite films exceeded that of pure PEEK film, whereas an opposite trend was observed for elongation at break, which was explained as follows, on the one hand, MWCNTs increase the strength of composite films; on the other hand, the addition of MWCNTs decreases matrix crystallinity and increases the amount of structural defects.13 Overall, the prepared composite films exhibited relatively good mechanical properties, which was attributed to the homogeneous dispersion and good interfacial adhesion discussed above. The densities of PEEK and its composite films gradually increased with increasing filler content but did not exceed 1.34 g cm−3 for all films. Compared to conventional metal-based EMI shielding materials such as nickel–copper alloys with densities as high as 8.6 g cm−3, PEEK/wrapped MWCNT/GPPS1.0 composite films exhibited the advantage of combining low density with relatively high EMI SE.
The EMI SE of PEEK/wrapped MWCNT/GPPS1.0 composite films were measured at frequencies of 8.2–40 GHz to evaluate the effects of the wrapped MWCNTs and GPPS, which was determined by scattering parameters, according to the equation:
Material | Frequency (GHz) | SE (dB) | SSEa (dB mm−1) | Thickness (mm) | Tensile strength (MPa) | T5%b (°C) | Reference |
---|---|---|---|---|---|---|---|
a SSE: specific EMI SE, which was divided by the thickness of the composite film.b 5% weight loss temperature in TGA test.c PANI: polyaniline; PS: polystyrene.d PVB: polyvinyl butyral.e PC: polycarbonate.f PMMA: polymethyl methacrylate. | |||||||
PEEK/wrapped MWCNT/GPPS1.0 | 8.2–12.4 | ∼10.5 | 58.3 | 0.18 | 101 | 586 | This work |
40 | 16.2 | 90.0 | 0.18 | ||||
PEEK/wrapped MWCNT | 12.0–18.0 | ∼55 | ∼27.5 | 2 | 91 | 583 | 13 |
Fe3O4@PANI/polyazomethine/PEEK | 2.0–18.0 | ∼10 | 5 | 2 | 11.17 | ∼300 | 28 |
PANI–CNT/PSc | 12.4–18 | ∼24 | 24 | 1 | — | — | 29 |
PS–PANI–clay | 8.0 | 16.2 | 16.2 | 1 | 70.6 | ∼320 | 30 |
PVB–PANI nanofiberd | 8.2–12.4 | ∼26 | 33.3 | 0.78 | — | — | 31 |
Poly lactide/graphene nanoplatelet | 9.0 | ∼14.3 | 9.53 | 1.5 | — | — | 32 |
PC/MWCNTe | 17.5 | 27.2 | 9 | 3 | 72 | — | 33 |
PMMAf/MWCNT | 8.0–12.0 | 18 | 60.0 | 0.3 | 30 | ∼200 | 34 |
In addition, the prepared PEEK/wrapped MWCNT/GPPS1.0 composite film (9 wt% wrapped MWCNT) possessed high flexibility. As shown in Fig. 6a, the films can be easily wound into rolls and bent over a large angle, with no cracks and creases appearing after bending; moreover, due to the excellent flexibility, the film can be fold into various shapes, i.e., paper crane. The properties of composite films were determined by the dispersion of wrapped MWCNTs in the PEEK matrix, since the important features such as conductivity and EMI SE were disrupted by heterogeneity or filler aggregation. Fig. 6b shows the cross-section SEM image of PEEK/wrapped MWCNT/GPPS1.0 composite film (9 wt% wrapped MWCNT) with a typical roll and composite film fracture morphology, revealing that the film possessed smooth surface and wrapped MWCNTs were almost uniformly dispersed in PEEK matrix, with no agglomeration or entanglement observed. Besides, no open-ring holes or voids were detected around wrapped MWCNTs, indicating good compatibility and interfacial adhesion between the filler and the matrix. Thus, the relatively good conductivity and EMI SE of PEEK/wrapped MWCNT/GPPS1.0 composite film could be attributed to the addition of a well-dispersible conductive filler (wrapped MWCNTs) and a high-temperature lubricant (GPPS).
Footnote |
† Electronic supplementary information (ESI) available: The dimensions of film samples in EMI shielding test; TGA curves of PEEK/MWCNT composites with different GPPS contents; comparisons of AC conductivities and thermal stabilities between PEEK/MWCNT/GPPS1.0 and PEEK/wrapped MWCNT/GPPS1.0 composite films; the detailed EMI SE and specific EMI SE of PEEK/wrapped MWCNT/GPPS1.0 film (9 wt% wrapped MWCNT) at various frequencies. See DOI: 10.1039/c7ra11675f |
This journal is © The Royal Society of Chemistry 2018 |