Andrea Cappelli*a,
Marco Paolinoa,
Annalisa Realea,
Vincenzo Razzanoa,
Giorgio Griscia,
Germano Giuliania,
Alessandro Donatia,
Claudia Bonechia,
Stefania Lamponia,
Raniero Mendichib,
Salvatore Battiatoc,
Filippo Samperic,
Francesco Makovecd,
Mariano Licciardief,
Lorenzo Depaug and
Chiara Bottab
aDipartimento di Biotecnologie, Chimica e Farmacia and European Research Centre for Drug Discovery and Development, Università degli Studi di Siena, Via A. Moro 2, 53100 Siena, Italy. E-mail: andrea.cappelli@unisi.it; Tel: +39 0577 234320
bIstituto per lo Studio delle Macromolecole (CNR), Via A. Corti 12, 20133 Milano, Italy
cIstituto per i Polimeri, Compositi e Biomateriali (IPCB) U.O.S. di Catania, CNR, Via Gaifami 18, 95126 Catania, Italy
dRottapharm Biotech, Via Valosa di Sopra 9, 20900 Monza, Italy
eDipartimento di Scienze e Tecnologie Biologiche, Chimiche e Farmaceutiche (STEBICEF), Università degli Studi di Palermo, Via Archirafi 32, 90123 Palermo, Italy
fMediterranean Center for Human Health Advanced Biotechnologies (CHAB), University of Palermo, Italy
gDipartimento di Biotecnologie Mediche, Università degli Studi di Siena, Via A. Moro 2, 53100 Siena, Italy
First published on 6th February 2018
In order to develop a technology platform based on two natural compounds from biorenewable resources, a short series of hyaluronan (HA) copolymers grafted with propargylated ferulic acid (HA–FA–Pg) were designed and synthesized to show different grafting degree values and their optical properties were characterized in comparison with reference compounds containing the same ferulate fluorophore. Interestingly, these studies revealed that the ferulate fluorophore was quite sensitive to the restriction of intramolecular motion and its introduction into the rigid HA backbone, as in HA–FA–Pg graft copolymers, led to higher photoluminescence quantum yield values than those obtained with the isolated fluorophore. Thus, the propargyl groups of HA–FA–Pg derivatives were exploited in the coupling with oleic acid through a biocompatible nona(ethylene glycol) spacer as an example of the possible applications of this technology platform. The resulting HA–FA–NEG–OA materials showed self-assembling capabilities in aqueous environment. Furthermore, HA–FA–NEG–OA derivatives have been shown to interact with phospholipid bilayers both in liposomes and living cells, retaining their fluorogenic properties and showing a high degree of cytocompatibility and for this reason they were proposed as potential biocompatible self-assembled aggregates forming new materials for biomedical applications.
The glycosaminoglycan hyaluronic acid (HA, hyaluronan) plays important roles in human body. Among them, HA forms a pericellular coat playing a pivotal role in the early stages of cell adhesion18 by interacting with CD44 receptor.19,20 This receptor is an ubiquitous protein possessing an extracellular portion called hyaluronan binding domain and has been described to be expressed in high density in tumor tissues.21
In our previous studies, the HA backbone was grafted with variable densities of FA residues to afford HA–FA graft copolymers in the aim of combining the intriguing properties of the two natural compounds.22,23 Furthermore, a tri-component polymer brush was designed by functionalization of a polybenzofulvene derivative with nona(ethylene glycol) (NEG) side chains terminated with low molecular weight hyaluronic acid macromolecules.24,25 This material was prepared by means of a convergent approach employing a copper(I)-catalyzed azide–alkyne 1,3-dipolar cycloaddition (CuAAC) of the suitable polybenzofulvene derivative (the azide component) with the hyaluronan derivative HA–FA–Pg (Fig. 1) bearing propargyl groups bound to HA backbone through FA fluorophores.24
In order to develop a technology platform based on two natural compounds from biorenewable resources, we prepared a short series of hyaluronan-based graft copolymers (HA–FA–Pg) showing different grafting degree (GD) values and we studied their optical properties. In the attempt to demonstrate the usefulness of the technology platform, the propargyl groups of HA–FA–Pg derivatives were exploited in the CuAAC coupling with alpha-azido-omega-oleic amide nona(ethylene glycol) (compound 3, azido-NEG–OA) to obtain amphiphilic HA derivatives (i.e. HA–FA–NEG–OA). The obtained HA–FA–NEG–OA showed potential self-assembling abilities in aqueous environment and for this reason was herein exhaustively characterized and proposed as biocompatible material with high potentiality in biomedical applications (i.e. in drug delivery).
Entry | Copolymer | HA (g) | HA (mmol) | 1/HA ratio (%) | Grafting degreea (%) | Convers.b (%) |
---|---|---|---|---|---|---|
a A rough estimate of the grafting degree was made by 1H NMR spectroscopy after hydrolysis with NaOD in D2O as described in ref. 22.b The conversion into ferulate was calculated from the substitution degree and stoichiometric ratio 1/HA.c See ref. 24. | ||||||
1 | HA–FA–Pg-01 | 0.50 | 1.32 | 25 | 20 | 80 |
2 | HA–FA–Pg-02 | 0.50 | 1.32 | 25 | 18 | 72 |
3 | HA–FA–Pg-03 | 0.50 | 1.32 | 25 | 20 | 80 |
4 | HA–FA–Pg-1F | 0.39 | 1.03 | 50 | 33 | 66 |
5 | HA–FA–Pg-2F | 0.50 | 1.32 | 50 | 35 | 70 |
6 | HA–FA–Pg-3Fc | 1.0 | 2.64 | 25 | 20 | 80 |
7 | HA–FA–Pg-4F | 1.0 | 2.64 | 12.5 | 10 | 80 |
Fig. 2 Enlarged sections of the MALDI-TOF mass spectra (negative ions) of the samples: (a) HA–FA–Pg-2F; (b) HA–FA–Pg-3F; (c) HA–FA–Pg-4F. |
The MALS calibration constant was calculated using toluene as standard by assuming a Rayleigh factor of 1.406 × 10−5 cm−1. The MALS angular normalization was performed by measuring the scattering intensity of a concentrated solution of a pullulan polysaccharide with narrow molecular weight distribution (MWD, Mp = 12 kg mol−1, Mw/Mn < 1.03, Rg = ≈2.1 nm) assumed to act as an isotropic scatterer. It is known that the on-line MALS detector measures, for each polymeric fraction eluted from the SEC columns, the molecular weight (M) and when the angular dependence of the scattered light is experimentally measurable also the molecular size generally known as radius of gyration (Rg). The SEC-MALS system was described in detail elsewhere.26,27
The differential refractive index increment of the polymers with respect to the solvent mixture was measured off-line by a Chromatix KMX-16 differential refractometer.
PANC-1 (human pancreas adenocarcinoma) cells for confocal microscopy studies were obtained from American Type Collection and cultured as described above.
Scheme 1 Preparation of the HA–FA–Pg derivatives. Reagents: (i) HCONH2, TEA. Substituents: R = H or C2H5. |
The functionalization reaction was carried out in formamide as the solvent and in the presence of triethylamine (TEA) as the base to afford the desired graft copolymer HA–FA–Pg.24 The stoichiometric ratio between 1 and HA (i.e. 1/HA ratio, Table 1) was varied from 50 to 12.5% with a number of replicates in 1/HA ratios of 25% and 50% in the aim of evaluating the reproducibility of the molar grafting degree (GD) observed. The isolation of the copolymer from the reaction mixture was performed by precipitation with acetone to obtain samples as white solids.
The analysis of the data reported in Table 1 demonstrate that GD value can be regulated in the range 10–35% by using the correct 1/HA stoichiometric ratio, with high and quite reproducible conversion values (i.e. 60–80%).
Some selected HA–FA–Pg samples were then used in the CuAAC coupling with alpha-azido-omega-oleic amide nona(ethylene glycol) (azido-NEG–OA, 3) to obtain HA derivatives (i.e. HA–FA–NEG–OA) as depicted in Scheme 2.
The copper(I) catalyst was generated in situ with CuSO4/sodium ascorbate in order to perform the CuAAC coupling under very mild conditions. The coupling reaction was carried out by using two HA–FA–Pg samples showing different grafting degrees (i.e. about 20% corresponding to four propargyl groups per HA macromolecule in HA–FA–Pg-3F, and about 35% corresponding to eight propargyl groups per HA macromolecule in HA–FA–Pg-2F) in the aim of obtaining HA–FA–NEG–OA derivatives bearing different densities of OA side chains pending from the HA backbone (i.e. about four in HA–FA–NEG–OA–4, and about eight in HA–FA–NEG–OA–8).
Finally, compound FA–NEG–OA and its methyl ester precursor 5 were synthesized as described in Scheme 3 in order to be used as model compounds.
Scheme 3 Synthesis of model compounds 5 and FA–NEG–OA. Reagents: (i) CuSO4, sodium ascorbate, tert-BuOH, H2O; (ii) NaOH, H2O, C2H5OH. |
Sample | dn/dc (mL g−1) | Mp (kg mol−1) | Mw (kg mol−1) | Mw/Mn | Rec. mas.a (%) | Graftingb (%) |
---|---|---|---|---|---|---|
a Recovered mass: the fraction of the polymeric sample eluting from the SEC columns.b A rough estimate of the grafting degree was made by 1H NMR spectroscopy after hydrolysis with NaOD in D2O as described in ref. 22. | ||||||
HA | 0.116 | 8.5 | 8.7 | 1.53 | 70 | 0 |
HA–FA–Pg-1F | 0.125 | 8.4 | 7.3 | 1.40 | 61 | 33 |
HA–FA–Pg-2F | 0.125 | 7.0 | 6.3 | 1.34 | 59 | 35 |
HA–FA–Pg-3F | 0.122 | 6.8 | 6.5 | 1.45 | 56 | 20 |
HA–FA–Pg-4F | 0.120 | 7.0 | 6.7 | 1.22 | 66 | 10 |
In consideration of the complex copolymer structure and the unusual SEC solvent mixture, the recovered mass values of the samples were relative high and substantially adequate for estimating the whole MWD of the copolymers, particularly after the derivatization reactions. Consequently, the SEC-MALS results in Table 2 provide interesting and very useful information for the native HA and the HA–FA–Pg derivatives.
The molecular weight of the starting HA sample was relatively low for a HA polysaccharide (Mw average about 8.7 kg mol−1) and the MWD was substantially broad (Mw/Mn about 1.5). On the whole, in consequence of grafting the MWD of HA–FA–Pg derivatives change only a little (i.e. the Mw average decrease from 8.7 kg mol−1 of the starting HA to 6.3 kg mol−1 of the HA–FA–Pg-2F derivative showing 35% of grafting). During derivatization reactions two molecular weight tendencies are simultaneously working in opposite ways: (1) a molecular weight decrease produced by an eventual degradation; (2) a molecular weight increase produced by the grafting. The data reported in Table 2 demonstrated that degradation of HA starting biopolymer is relatively low also for high level of grafting. Furthermore, the dn/dc values appeared to be quite well related with the grafting degree and this result substantially confirmed the estimation of the grafting.
Functionalized HA–FA–Pg samples (i.e. HA–FA–Pg-2F, HA–FA–Pg-3F, and HA–FA–Pg-4F) were characterized by MALDI-TOF MS in negative-ion mode using DHB or DCTB as the matrix. The best mass resolved mass spectra of the HA–FA–Pg-3F and HA–FA–Pg-4F samples were recorded using the DHB as the matrix, and the DCTB one for the HA–FA–Pg-2F derivative. As previously reported,24 the mass spectrum of starting HA showed, in the mass range m/z 2500–10000 Da, a series of clusters corresponding to the even-numbered HA oligosaccharides (7- to 23-mers, species An). On the other hand, complex mass spectra were obtained in the case of the hyaluronan graft copolymers HA–FA–Pg-2F, HA–FA–Pg-3F, and HA–FA–Pg-4F, which shows a series of cluster of peaks in the mass range m/z 3500–10000. Enlarged sections of these mass spectra are reported in Fig. 2 together with the structural assignment. The analysis of the spectra suggested that the most intense peaks belong to the expected graft copolymer chains (species Ax,y). In particular, most of the copolymer chains present along the backbone: 6–8 ferulate residues in the case of HA–FA–Pg-2F, 4–5 ferulate residues in the case of HA–FA–Pg-3F, 2–3 ferulate residues in the case of HA–FA–Pg-4F. The corresponding copolymer chains containing ethyl ester groups (species A′x,y) were also revealed in accord to the mass spectrum of the initial HA sample. The mass spectra revealed also the presence of unfunctionalized oligosaccharides, in particular in the case of the HA–FA–Pg-3F and the HA–FA–Pg-4F samples (Fig. 2). Thus, the MALDI mass spectra confirmed the formation of the reactive functionalized oligosaccharides.
The 1H NMR spectra indeed showed, beside the typical profile of HA in the up-field region, signals attributed to the propargylated FA residues in the down-field region of the recorded spectra. Moreover, the relative intensity of the signals in the aromatic region increased from HA–FA–Pg-4F (grafting degree around 10%) to HA–FA–Pg-3F (grafting degree around 20%) and HA–FA–Pg-2F (grafting degree around 35%) with the increase of the grafting degree. This observation along with the broadness of the typical signal pattern in the aromatic region supported further the occurrence of the functionalization.
The more resolved spectral lines allowed a more detailed comparison of the 13C NMR spectra (Fig. 4) to be done.
The assignment of the 13C NMR spectra of HA and HA–FA–Pg samples was performed as previously described.24 In agreement with that observed in the analysis of 1H NMR spectra, the relative intensity of the signals attributed to propargylated FA residues increased with the increase of the grafting degree, which appeared to play a negligible role in modulating the shoulder of the signals attributed to anomeric C – a carbon atom of HA.
In order to evaluate the occurrence of the click chemistry coupling between the selected HA–FA–Pg samples (i.e. HA–FA–Pg-2F and HA–FA–Pg-3F) leading HA–FA–NEG–OA derivatives (i.e. HA–FA–NEG–OA–8 and HA–FA–NEG–OA–4, respectively), the 1H and 13C NMR spectra of HA–FA–NEG–OA–4 were analyzed in comparison with those of its synthetic precursor and HA–FA–Pg-3F (Fig. 5 and 6) and of the model compound FA–NEG–OA, which was extensively characterized by means 1D and 2D NMR techniques. In this way, we were able to assign all the signals of the complex spectra obtained with HA–FA–NEG–OA materials (see ESI†).
In fact, the 1H NMR spectrum of the HA–FA–NEG–OA–4 material (Fig. 5) appeared to be composed by a multitude of signals deriving from the integration of discrete signal patterns relevant to the different components of the material.
Interestingly, the disappearance of the peak at 2.91 ppm attributed to acetylene proton of HA–FA–Pg-3F and the appearance of a new peak at 8.02 in the spectrum of HA–FA–NEG–OA–4 material supported the transformation of the alkyne moiety into the triazole one as it usually occurs in CuAAC coupling reaction. Therefore, this observation was considered to be a strong evidence of the structure of FA–NEG–OA-4 material. Furthermore, a significant line broadening was observed in the signals attributed to the aromatic and acrylic protons of FA moiety.
Similarly, the 13C NMR spectrum of the HA–FA–NEG–OA–4 material (Fig. 6) resulted by the combination of the signal patterns relevant to the different components of the material. Among them, the signals attributed to the low molecular weight HA ribbons and to NEG side chains dominated the spectrum, with the one attributed oleic acid moiety playing a relatively minor role, and the ones belonging to the aromatic carbon atoms of ferulate component being lost in the baseline modulations. In agreement with previous observations,24 we assumed that owing to its role of linker between the two macromolecular components (i.e. HA and OEG–OA), the FA moiety suffered from a reduced mobility, which could produce a pronounced line broadening as already observed in the 1H NMR spectrum in Fig. 5.
Nevertheless, the persistence of the signal attributed to the ferulate methoxy C-A (at about 55.6 ppm) and the apparent shift of both the one attributed to the ferulate propargyl C-B (at about 56.4 ppm) and the one attributed to the ferulate propargyl carbons C-D and C-C (at about 76 ppm) were assumed to confirm the occurrence of the CuAAC coupling reaction.
The comparison of the 1H NMR spectra obtained with increasing concentrations of HA–FA–NEG–OA–4 in D2O (Fig. 7) showed a gradual broadening, which suggested a tendency towards aggregation of this material.
This result led us to assume the formation of colloidal water dispersions with HA–FA–NEG–OA–4 in the form of micelles with a hydrophobic core constituted by the oleic residues. The high field (900 MHz) NOESY spectrum (Fig. 8) performed on the water dispersions of the material showed the presence of strong dipolar interactions among different portions of the macromolecules, which should be far in extended conformations, but were evidently near from each other in the 3D space.
Fig. 8 High field (900 MHz TCI cryo) NOESY spectrum (mixing time 200 ms) performed on the water (i.e. D2O, with water suppression) dispersions of HA–FA–NEG–OA–4 material. |
This result suggested the existence of a strong entanglement of the side chain components (both the lipophilic oleic one and the amphiphilic NEG one) in the core of the micelles, which exposed on their surface the hydrophilic side of the hyaluronan ribbon as suggested by the apparent lack of dipolar interactions of the acetamide methyl group (sharp singlet at 1.92 ppm) with the side chain components.
The relative sign of cross-peaks in a NOESY spectrum depends on the rotational correlation time, i.e. if the rotational correlation time of the molecules is long, the diagonal and cross-peaks have same signs.30 This result allowed assertion that the HA–FA–NEG–OA–4 experienced a slower motion in solutions confirming the aggregation processes.
At high concentration the HA–FA–NEG–OA–4 forms very large aggregates, whose polydispersity index (PDI) was reasonable even if quite high. In this case, the distribution curve obtained from Laplace reversal for such large diameter values may contain artifacts. The aggregate size analysis was, furthermore, limited to the restrictions of DLS, where the aggregate must remain small enough for Brownian forces to dominate gravitational force, preventing sedimentation, which for polymeric particles is generally considered to be 1000 nm.31 The high polydispersity indexes revealed that the systems were not perfectly monodispersed. The size decrease with concentration and this experimental data highlight that the macromolecule aggregate structure was similar to spherical or a worm-like micelles.
HA–FA–NEG–OA–8 at the maximum tested concentration of 30 mg mL−1 had two main distributions, whose data were not, however, very reproducible. This is typical of polymeric solutions in which macromolecules do not have a well-defined form. HA–FA–NEG–OA–8 produced smaller aggregate than HA–FA–NEG–OA–4. However, these experimental data suggest that the both HA–FA–NEG–OA materials in solution were able to form aggregates such as spherical or worm-like micelles.
Compd | Solutiona,b,c | Solidd,e | |||
---|---|---|---|---|---|
λab (nm) | λem (nm) | PLQY (%) | λem (nm) | PLQY (%) | |
a Dichloromethane.b Methanol.c Water.d Spin.e Cast. | |||||
6 | 290, 320a,b | 405b | 0.34b | 430e (450d) | <0.1 |
4 | 290, 320a,b | 390a (410b) | 0.24a (0.34b) | 370e (390d) | 4.4 |
FA–NEG–OA | 290, 320a | 400a | 0.28a | ||
5 | 290, 320a | 390a | 0.24a | 400e | <0.1 |
HA–FA–Pg-2F | 290, 320c | 450c | 0.68c | 420e | 7.6 |
HA–FA–Pg-3F | 290, 320c | 445c | 0.75c | 420e | 5.5 |
HA–FA–Pg-4F | 290, 320c | 445c | 0.83c | 420e | 7.3 |
HA–FA–NEG–OA–4 | 290, 320c | 440c | 0.79c | 420e | 2.9 |
HA–FA–NEG–OA–8 | 290, 320c | 430c | 0.87c | 415e | 4.8 |
The absorption/emission features of ferulic acid have been previously demonstrated to be affected by solvent polarity and pH. In fact, FA possesses in its structure two acidic moiety showing well distinct pKa values (4.4 and 9.0, see ref. 5). The neutral FA molecule is barely fluorescent, whereas the singly-ionized form is twofold more fluorescent (excitation maximum at 290–310 nm and emission maximum around 420 nm), and the doubly-ionized one is the most emissive specie (at pH = 10, the excitation maximum was shifted to 345 nm and emission maximum to 470 nm, see ref. 5). Furthermore, the decrease in solvent polarity was reported to produce decreases in the excitation, emission, and Stokes shift of FA solutions (i.e. the blue-green fluorescence was quenched by 80% in chloroform with respect to water, see ref. 5).
By the propargylation of the phenolic OH of FA as in compound 6, the less acidic group of FA is lost, and compound 6 shows absorption maxima similar to those reported for FA and slightly sensitive to solvent polarity (methanol: 235, 290 and 318 nm Fig. 10; dichloromethane: 238, 295 and 324 nm, see ESI†). On the other hand, the corresponding ester 4, lacking both the ionisable groups, shows very similar absorption spectra in the solvents with well-distinct polarities such as dichloromethane and methanol, with bands peaked at 238, 292 and 319 nm (see Fig. 10 and ESI†).
Fig. 10 Absorption (left) and emission (right) spectra of ester 4 in dichloromethane and acid 6 in methanol at 10−5 M. |
The molar extinction coefficient of ester 4 (i.e. 21817 L mol−1 cm−1) was found to be well related to the one described for soyamide ferulate (i.e. 19705 L mol−1 cm−1).32
Ester 4 and the corresponding acid 6 showed similar emissive features in solution with PL maxima centred at 410 nm and 406 nm in methanol for 4 and 6, respectively, while the spectrum shifted at 388 nm for 4 in dichloromethane, in agreement with a reduction of the Stokes shift in solvents with lower polarities, as already reported for FA solutions. They were weakly emissive in solution (PLQY = 0.24% for ester 4 in dichloromethane and 0.34% for both ester 4 and acid 6 in methanol), but a significant increase in the PLQY (i.e. 4.4%) was observed in the films obtained with ester 4 while the emission of acid 6 in the solid state is very low (see Table 3, Fig. 11).
Fig. 11 Emission spectra of ester 4 in the solid state, film obtained by spin coating compared to the film obtained by casting. |
In order to better understand the emissive properties of the two compounds 4 and 6 we cooled their diluted solutions down to 77 K in order to block the molecular motions often responsible for the lack of emission of aggregation-induced emission (AIE) molecules in solution.33,34 We observed, for both compounds 4 and 6, a strong increase (a factor of about 50–80) in the emission intensity when the solutions are frozen at 77 K (see ESI†). This result demonstrates that, by restricting their molecular motions, both 4 and 6 compounds emit strongly, while upon aggregation only compound 4 displays a sensitive emission enhancement. This fact evidences the importance of a proper molecular packing for the exploitation of the AIE properties of this class of fluorogens, as observed for some closely related cinnamic derivatives.35 Therefore, compound 4 showed a typical AIE behavior,36,37 with photoluminescence quantum yields in the solid state increased by one order of magnitude with respect to the corresponding values measured in solution. Furthermore, we note that the emission spectra in the solid state depend on the film deposition procedure. When the film is obtained by casting the solution a better organization of the molecules is usually obtained with respect to the spincoating deposition, which causes a rapid evaporation of the solvent. As a result, the emission of the cast film displays a sharper and better structured spectrum while that of the spincoated film is closer to the solution one.
This result stimulated our interest in evaluating the effects of the introduction of ferulate fluorogen in the rigid HA backbone as in HA–FA–Pg graft copolymers. The photophysical features of three HA–FA–Pg samples showing different grafting degrees were investigated both in the water solutions and in the solid state. The absorption spectra of the polymeric materials were dominated by the absorption of the ferulate fluorophores with maxima perfectly matching with those of ester 4 (290 and 320 nm), whereas a significant red shift was observed in the emission spectra recorded with the water solutions of HA–FA–Pg, as expected due to the high polarity of the solvent (Table 3, Fig. 12).
The PLQY values measured with the water solutions of HA–FA–Pg samples resulted higher (in the range of 0.68–0.83%) than of the corresponding value obtained with the solution of ester 4 in dichloromethane (0.24%). This effect was retained also when HA–FA–NEG–OA were compared with the corresponding model compounds 5 and FA–NEG–OA and could be rationalized with the decrease of the mobility of the ferulate fluorogen as suggested by NMR studies.
A further significant increase in the PLQY was observed in the solid-state samples (i.e. cast films) of the polymeric materials, which showed PLQY values (in the range 2.9–7.6%) sufficiently promising for a further characterization of these materials in view of their potential biomedical applications.
Unilamellar vesicles showing sub-micrometer dimensions (SUV) were prepared by standard procedures, and the mean diameters, polydispersity indexes and ζ-potential of the DOPC/DOPE liposomes with and without HA–FA–NEG–OA–8 (Table 4) indicated that insertion of the material into liposomes led to an increase in the mean diameter of vesicles. The vesicle diameter changed significantly after the addition (143.9 ± 6.8 nm). The low polydispersity indexes of plain and loaded systems revealed that liposomes were not substantially altered by interaction with HA–FA–NEG–OA–8. Indeed, synthesized liposomes remained fairly monodispersed.
Liposome composition | Size ± SD (nm) | PDI | ζ potential ± SD (mV) |
---|---|---|---|
DOPC/DOPE | 105.7 ± 11.0 | 0.16 | −13.6 ± 4.8 |
DOPC/DOPE + HA–FA–NEG–OA–8 | 143.9 ± 6.8 | 0.18 | −41.0 ± 10.3 |
Plain DOPC/DOPE liposomes had a small negative ζ-potential, though the net polar head charge of zwitterionic phospholipids is zero. The insertion of HA–FA–NEG–OA–8 changes the zeta potential to more negative values (−41.0 mV) suggesting that the system is chemically stable and no aggregation or flocculation processes may occur in the solution.
Thus, the photophysical characterization of HA–FA–NEG–OA–8 derivative was deepened in the phospholipid environment, both in the SUV dispersions in water and in the solid state of the cast films. The results (see ESI†) suggested that the interaction of HA–FA–NEG–OA–8 derivative with phospholipid bilayers produced negligible effects in the photophysical features of HA–FA–NEG–OA derivatives maintaining the AIE properties of the fluorogen.
Moreover, the results obtained demonstrated the high degree of in vitro cytocompatibility of the test materials which did not interfere with cell viability of both immortalized cells, such as 3T3 fibroblasts, and primary human cells, such as chondrocytes.
Moreover, the internalization of both the polymeric materials (i.e. HA–FA–NEG–OA–4 and HA–FA–NEG–OA–8) was further confirmed by confocal microscopy in PANC-1 cells with membrane labelling by means of FITC-conjugated lectin in order to better visualize the cellular surface (Fig. 15).
In fact, a clear fluorescence signal was observed in the cytoplasm of the cells treated with HA–FA–NEG–OA–4 or HA–FA–NEG–OA–8 materials that was attributed to ferulic fluorogen internalized into PANC-1 cells after 30 min of contact and 2 h of internalization. This result suggests for HA–FA–NEG–OA materials potential applications in intracellular delivery.
In the attempt to demonstrate the usefulness of the technology platform, the propargyl groups of HA–FA–Pg derivatives were exploited in the coupling with a third natural component from biorenewable resources (i.e. oleic acid) through a biocompatible spacer composed of nine monomeric units of ethylene glycol. The resulting HA–FA–NEG–OA derivatives showed self-assembling capabilities in aqueous environment and for this reason were characterized as potential biocompatible self-assembled aggregate forming material for biomedical applications. In particular, HA–FA–NEG–OA derivatives were demonstrated to interact with phospholipid bilayers both in liposomes and living cells retaining the fluorogenic properties and showing a high degree of cytocompatibility.
On the basis of its high modularity, we envisioned for this technology platform a broad applicability. In fact, a broad range of polymeric carriers can be used beside to different fatty acid residues and oligo(ethylene glycol) spacers, with ferulate playing the central role of natural small molecule fluorogenic clickable linker.
Footnote |
† Electronic supplementary information (ESI) available: Synthetic procedures for the preparation of azide 3 and of model compounds 5 and FA–NEG–OA; 1H NMR spectrum of HA–FA–NEG–OA–8 compared with that of HA–FA–NEG–OA–4; 13C NMR spectrum obtained with HA–FA–NEG–OA–4 derivative compared with those obtained with HA, HA–FA–Pg-3F, and model compound FA–NEG–OA; absorption spectra of compounds 4 and 6. See DOI: 10.1039/c7ra12543g |