Qing Liua,
Ning Chena,
Shibing Bai*a and
Wenzhi Lib
aState Key Laboratory of Polymer Materials Engineering, Polymer Research Institute of Sichuan University, Chengdu 610065, China. E-mail: baishibing@scu.edu.cn; Fax: +86-28-85402465; Tel: +86-28-85405136
bState Key Laboratory of Special Functional Water Proof Materials, Beijing Oriental Yuhong Waterproof Technology Co., Ltd, Beijing 100000, China
First published on 12th January 2018
The thermal processing of poly(vinyl alcohol) (PVA) is a big challenge worldwide. In this article, silver nitrate (AgNO3), which can combine with the hydroxyl groups of PVA and water, was introduced to further improve the thermal processability of the poly(vinyl alcohol)/water system. The water states, thermal performance, and rheological properties of PVA modified by AgNO3 were investigated. The results showed that with the increasing of AgNO3 content, the content of bound water in system increased ascribing to the interaction among PVA, water and AgNO3, indicating that the bondage of PVA matrix on water enhanced, thus retarding the tempestuous evaporation of water in system during melt process and making more water remain in system to play the role of plasticizer. Meanwhile, that AgNO3 combined with the hydroxyl groups of PVA further weakened the self-hydrogen bonding of PVA, guaranteeing a lower melting point and higher decomposition temperature, and broadening the thermal processing window. The rheological properties of the modified PVA system showed that the torque and die pressure of the modified PVA system turned to stabilization during melt processing, testifying that the thermal processability of the PVA/water system was largely improved.
Generally, the key point to realize thermal processing of PVA is to obtain a thermal processing window,1 by means of destroying the self-hydrogen bonding of PVA and decreasing its melting point, which can be realized by addition of plasticizers, chemical modification3 or blending4–8 etc. Among these, using plasticizers for modifying PVA is a simple and effective way to extend the gap between the melting point and the decomposition temperature of PVA. The common plasticizers for modifying PVA are water,1,9,10 polyols,9,11–13 amides,9,14 esters,10 metal salts,15,16 etc. These plasticizers could form hydrogen bonding with –OH of PVA, decrease the original inter and/or intra-molecular hydrogen bonding of PVA and then destroy the structural regularity and degree of crystallinity, making the melting point of PVA decrease.1 Consequently, thermal processing window is obtained and thermal processing of PVA is able to be realized. Water is popular and most suitable one for PVA because of its clear and low cost. But it, whose boiling point is low (∼100 °C), is easy to evaporate and cause unstable flow even foaming during thermal processing. Therefore, how to control water evaporation and further decrease the interaction between PVA molecules are quite important for the stable thermal process of water plasticized PVA. Wang et al.17 selected boric acid as a modifier to investigate water states and thermal processability of modified PVA, getting that boric acid inhibited the intense water evaporation during the melting process and improved the processing stability of modified PVA. However, boric acid cannot be easily got rid of and has poisonousness.18
Ag+ would vanish and turn into Ag nanoparticles when heating19 or UV irradiating,20 which endow PVA/Ag composites with antibacterial property,21 optical applications,20 biosensors22 and so on. Besides, Ag+ contains several vacant orbital, which could help Ag+ adopt lone pair electrons.19,23–25 So, Ag+ owns capacity to adopt electrons provided by hydroxyl-oxygen atom of PVA and water. Huang et al.25 indicated that Ag+ could combine with two hydroxyl of PVA and form PVA–Ag+ chelate, this structure destroy the original inter and/or intra-molecular hydrogen bonding of PVA and weaken intermolecular forces, eventually reducing its melting point. Furthermore, some Ag+ also could combine with water to form H2O–Ag+ chelate which could constrain water and even urge more water to play the role of plasticizer. In this work, AgNO3 was adopted as a modifier and its effects on stability of water and thermal processability of water plasticized PVA were systematically tested by DSC, rheology test and SEM analysis.
Curves of differential scanning calorimetry (DSC) were performed on a TA Q20 differential scanning calorimeter (TA Instruments, USA) under a flowing N2 with sample weighty about 6 mg. The samples were first cooled to −40 °C with liquid nitrogen, and then heated to 40 °C at a heating rate of 5 °C min−1. The thermal properties of modified PVA were also measured by heating from 40 °C to 255 °C at a heating rate of 10 °C min−1.
The torque and die pressure of modified PVA were measured on torque rheometer (RM-200C, Harbin Hapro electrical technology CO. LTD. Harbin China). The temperature was set at 100 °C, 150 °C and 150 °C, respectively.
The morphology of liquid-nitrogen-cryofractured section of specimens and the surface appearance of the extrudater were performed on scanning electron microscope (SEM) (FEI Instrument Co. Ltd, USA).
The metal salt silver ion (Ag+) has vacant orbital19,23–25 which makes it adopt lone pair electrons. So, Ag+ owns capacity to adopt the oxygen atom on the hydroxyl which were supplied by PVA and water, which makes it possible to combine with hydroxyl oxygen of water and PVA. Huang et al.25 indicated that Ag+ could combine with two hydroxyl of PVA, showed in Fig. 2. Therefore, in this PVA/water/AgNO3 system, PVA chelated Ag+ to destroy the hydrogen bonds of PVA, resulting in the changes of the peak of O–H, showed in Fig. 1. Moreover, some Ag+ also could combine with water to form H2O–Ag+ chelate. Therefore, the interactions in this PVA/water/AgNO3 system could be clearly presented in Fig. 3. AgNO3 combines with PVA together with water to build the chelates to break the self-hydrogen bonding of PVA and urge more water to play the role of plasticizer.
Fig. 2 Structure for PVA–Ag+ chelate proposed by Huang et al.25 |
Generally, water has three different associating states1,28 with hydrophilic polymers, i.e., free water, freezable bound water and non-freezing water. Compared with free water, having no interaction with PVA molecules and own the same melting point as pure water, freezable bound water has less closely association with hydroxy groups and its melting point is below 0 °C. Non-freezing water has directly interacting with the polar groups of hydrophilic polymer which have no detectable phase transition in the range of −40 °C to 20 °C. Both of them are also named as bound water. Accordingly, if the content of bound water in PVA can be increased, stable melt process should certainly be realized.
The states of water could be differentiated by low temperature differential scanning calorimetric (DSC) measurements, as shown in Fig. 4. Apparently, the pure PVA had none peak within the above cited range of temperatures, which indicated that pure PVA had no phase transformation occurred during this heating period. And the pure water had one intensely phase transformation peak corresponding to the melting point of ice water. Besides, the modified PVA had two visible endothermic peaks appeared in DSC curve at about T = −10 °C and T = 0 °C, which indicated that there existed more than two different kinds of water. The endothermic peak at lower temperature belonged to the phase transformation of freezable bound water, signing as peakfb, and the other one at higher temperature which overlapped with the phase transformation peak of pure water belonged to the phase transformation of free water, signing as peakf. The curves showed that the peak intensity of peakfb strengthened visibly once adding AgNO3, besides, with the increase of AgNO3 content, the peak intensity of peakfb enhanced substantially. Not only that, but the peakfb moved toward the direction of higher temperature as the amounts of AgNO3 increased.
Fig. 4 The heating curves of modified PVA: (a) deionized water; (b) pure PVA; (c) m-P0; (d) m-P0.1; (e) m-P0.5; (f) m-P1. |
To further explore the change of water states, the values of melting point (T) and melting enthalpy (−ΔH) of the modified PVA containing various AgNO3 amounts were recorded in Table 1. Observably, the melting enthalpy of peakfb and peakf changed with the amounts of AgNO3 increasing, that of freezable bound water increased from 32.3 J g−1 to 51.5 J g−1 and that of free water decreased from 18.0 J g−1 to 8.7 J g−1. Those results illustrated that the content of freezable bound water and free water which existed in modified PVA have changed with the amounts of AgNO3 increasing, in other words, AgNO3 has affected the water states of PVA/water system.
Ws (mg) | Tfb (°C) | −ΔHfb (J g−1) | Tf (°C) | −ΔHf (J g−1) | |
---|---|---|---|---|---|
a Ws: weight of modified PVA; Tfb: the melting point of freezable bound water; ΔHfb: melting enthalpy of freezable bound water; Tf: the melting point of free water; ΔHf: melting enthalpy of free water. | |||||
Pure water | 5.4 | — | — | 1.5 | 340.8 |
m-P0 | 7.2 | −11.0 | 32.3 | −0.4 | 18.0 |
m-P0.1 | 7.1 | −8.9 | 50.9 | −0.4 | 12.3 |
m-P0.5 | 7.6 | −7.8 | 47.0 | −0.3 | 12.0 |
m-P1 | 7.4 | −5.4 | 51.5 | −0.5 | 8.7 |
Furthermore, the weight of free water and freezable bound water of modified PVA could be calculated28 by the following equation eqn (1).
(1) |
Besides, the weight of non-freezing water of modified PVA could be calculated by the following equation eqn (2) because the total water in modified PVA consists of free water, freezable bound water and non-freezing water.
Wnf = Ww − Wf − Wfb | (2) |
The weight and content of vary types water of modified PVA which were calculated by eqn (1) and (2) were listed in the following Table 2.
Ws (mg) | Ww (mg) | Wfb (mg) | Wfb/Ww (%) | Wf (mg) | Wf/Ww (%) | Wnf (mg) | Wnf/Ww (%) | |
---|---|---|---|---|---|---|---|---|
a Ws: weight of modified PVA; Ww: weight of water in modified PVA; Wfb: weight of freezable bound water; Wf: weight of free water; Wnf: weight of non-freezing water. | ||||||||
Pure water | — | 5.40 | — | — | 5.4 | 100 | — | — |
m-P0 | 7.2 | 3.09 | 0.68 | 22.0 | 0.38 | 12.3 | 2.03 | 65.7 |
m-P0.1 | 7.1 | 3.05 | 1.06 | 34.7 | 0.26 | 8.5 | 1.73 | 56.7 |
m-P0.5 | 7.6 | 3.27 | 1.05 | 32.1 | 0.27 | 8.3 | 1.95 | 59.6 |
m-P1 | 7.4 | 3.18 | 1.12 | 35.2 | 0.19 | 5.9 | 1.87 | 58.8 |
It can be found from Table 2 that the content of freezable bound water and free water which existed in modified PVA did change when adding AgNO3. The content of freezable bound water increased from 22.0% to 34.7%, the content of free water decreased from 12.3% to 8.5% once adding AgNO3. Especially, the content of non-freezing water showed downtrend, rapidly decreased from 65.7% to 56.7% when adding AgNO3. Besides, the content of the three type water continued to change with the amounts of AgNO3 increasing.
Fig. 5 presented one kind of schematic structures of water in modified PVA system. Shown as Fig. 5(a), when slowly poured into PVA matrix, the water molecules would easily permeate PVA chain segments and preferentially combine with hydroxyl of PVA, developing the first water layer, this part water is non-freezing water. When added water reached this level that the combined points of the hydroxyl of PVA turned saturated, the hydrogen bond between water molecules and PVA were not formed any longer, the following water would combine with hydroxyl of the first water layer, developing the second and even more water layer, this part water called freezable bound water. With added water content continuing to increase, the water layer turn more, the PVA molecules did not restrain water any longer, there water showed almost no difference with pure water.
Fig. 5(b) showed AgNO3 replacing some first water layer to combine with the hydroxyl of PVA and meanwhile bond with water to form water layers. This schematic structure explained why content of non-freezing water decreased after adding AgNO3. And the interaction energies of H2O⋯Ag+, which is 10.38 Kcal mol−1,29 is further greater than that of H2O⋯H–OH, which is 6.8 Kcal mol−1,30 so Ag+ has greater force to bond water, restraining water and making more water layers stable.
The states of water existing in PVA reflected the interaction among water, Ag+ and PVA to some extent. Conversely, that AgNO3 combines with PVA and water to build the chelates changed the states of water.
Fig. 6 depicted the heating curves of modified PVA containing various AgNO3 amounts within the temperature range from 40 °C to 255 °C. It can be observed from Fig. 7 that the pure PVA had only one peak appeared at around T = 230 °C which belonged to the melting point of pure PVA. And the other four curves have similar profiles, two visible endothermic peaks can be seen at about T = 120 °C and T = 230 °C through the temperature monitored. The endothermic peak at lower temperature belonged to evaporation peak of water of modified PVA, signing as peakw and the other endothermic peak at higher temperature belonged to the melting peak of pure PVA, signing as peakp. As is showed in Fig. 7, the peakw moved to high temperature with the increase of AgNO3 content, the value of m-P0 was 113.5 °C, and that of m-P1 was 124.7 °C, increasing by 11.2 °C in comparison to m-P0. That is to say, the boiling point of water was indeed increased and the water which existed in modified PVA would be evaporated in higher temperature when AgNO3 was used to modify PVA. Besides, the peakw shape was broadened under the effect of AgNO3, meaning that water would be evaporated in the broad temperature range, this is beneficial to avoiding the formation of bubbles during thermal processing caused by the rapid evaporation of water. Therefore, under the influence of AgNO3, the evaporation behavior of water has been markedly improved.
Fig. 6 The heating curves of modified PVA: (a) pure PVA; (b) m-P0; (c) m-P0.1; (d) m-P0.5; (e) m-P1. |
The differences in the thermal processing rheological behaviors for modified PVA containing various AgNO3 amounts were reflected by the torque and die pressure. From Fig. 7(A1), it can be seen that the three torque curves all looked fluctuant to some extent, indicating that these melts were in a state of dynamic instability during thermal processing. The torque of m-P0 changed from 2.1 Nm to 8.9 Nm, fluctuating acutely. Whereas the value of torque turned placid once adding AgNO3 into PVA/water system, the torque of m-P0.1 and m-P1 changed from 3.9 Nm to 7.4 Nm, and that of m-P1 changed from 4.4 Nm to 8.5 Nm. Besides, Fig. 7(A2) showed the discrete distribution curves of torque, it can be clearly seen that these three discrete distribution curves looked like normal distribution which is the classic bell curve and the full width half maximum (FWHM) of m-P0 is 3.76 Nm, further exceeding that of m-P0.1 or m-P1. The results indicated that the addition of AgNO3 reduced the dispersion degree of torque and then made the melts more stable. The die pressure (Fig. 7(B)) had similar notable difference. Especially, the discrete distribution curve of m-P0, learning from Fig. 7(B2), showed two peaks. The results illustrated that the die pressure changed acutely and the melts were in unstable state when only using water to modify PVA. Obviously, the addition of AgNO3 made the melts stable in large extent and greatly changed the rheological properties and favored the thermal processing.
The morphology of extruded strips could intuitively reflect processability of composite materials. Fig. 8(a)–(c) showed the morphology of liquid-nitrogen-cryofractured section of extruded strips of modified PVA. Obviously, pores structures were only observed in Fig. 8(a), while the other two micro-morphology were continuous and compact. Fig. 8(d)–(f) described the surface appearance of the extrudater of modified PVA. It can be seen from Fig. 8 that the outlooks of the extruded strips of m-P0.1 and m-P1 were smooth, homogenous comparing with that of m-P0.
Fig. 8 The morphology of extruded strips of modified PVA: (a) and (d) m-P0; (b) and (e) m-P0.1; (c) and (f) m-P1. |
From the above results, further explanation can be given for the changes of thermal processing rheological behaviors of modified PVA. There is unavoidable that water would evaporate from the melts and then labilize the melts during extruding process. The addition of AgNO3 improved water evaporation behavior and avoided the melts unstable flow to some extent. Noticeably, during the practical processing, modified PVA is melted in a relative hermetic condition, e.g. in an extruder. The strong pressure induced by the rotation of screw will further inhibit the evaporation of water in modified PVA. As a result, more water remains in modified PVA acting as an effective plasticiser.
Substantially, the results benefited from the effect of Ag+, the addition of AgNO3 improved water evaporation behavior and avoided the melts unstable flow and generating bubbles which were brought about by water rapidly evaporation the during extruding process.
This journal is © The Royal Society of Chemistry 2018 |