W. W. Heab,
X. H. Yana,
Y. M. Lianga,
Y. F. Longa,
C. Pana,
J. L. Zhaoa,
L. Chena,
W. Xiong*c and
Q. X. Liu*d
aCity College, Wuhan University of Science and Technology, Wuhan, Hubei 430083, China
bState Key Laboratory of Materials Processing and Die & Mould Technology, Huazhong University of Science and Technology, Wuhan 430074, China
cWuhan National Laboratory for Optoelectronics, Huazhong University of Science and Technology, Wuhan 430074, China. E-mail: weixiong@hust.edu.cn
dUrban Construction College, Wuhan University of Science and Technology, Wuhan, Hubei 430081, China. E-mail: liuqiuxin1956@sohu.com
First published on 28th March 2018
Flexible transparent electrodes (TEs) are important for new electronic devices. This paper reports a scalable, cost effective Ag nanowires (AgNWs) TE, which is made of a SnO2·xH2O and AgNWs composite layer and a flexible polyethylene terephthalate (PET) bottom layer by a solution method at room temperature. The AgNWs/SnO2·xH2O composite TEs reveal a significant reduction of four orders in magnitude of sheet resistance, from 90 kΩ sq−1 to 12 Ω sq−1, while retaining transmittance of about 92% at 550 nm. This could be owing to the significant reduction of contact resistance for the weld-like junction of bound AgNWs. Compared with others, this method is characterized by filling gaps of the silver nanowire network with SnO2·xH2O. In addition, the adhesive forces between the AgNWs and the substrate are improved. This could be attributed to strong adhesion of SnO2·xH2O with the substrate. Moreover, this foldable transparent electrode is applicable for any non-planar surfaces and ultimately for future wearable optoelectronic devices.
However, pure AgNWs TEs also have three serious problems: low electrical conductivity, intrinsic nonconductive gaps which are not conductive and detrimental to the collection of carriers for the device, and poor adhesion to the substrate.
Firstly, pure AgNWs TEs still have electrical problems because of low contact between the AgNWs. As shown by experimental results, contact resistance of AgNWs (Rc) is the main source of sheet resistance (Rsh). The traditional methods for reducing Rc and improving conductivity are heating and pressing. Some of new methods are laser nano-welding, graphene coating, chemical annealing, plasmonic welding. However, all these methods only solve the problem of electrical conductivity but are helpless for addressing the other two issues.10–17
Secondly, pure AgNWs TEs have large area of blank space which is not conductive in AgNWs networks. In fact, AgNWs cover only 20% of the substrate. However, electrodes must cover all over the active areas for efficient charge extraction/injection because of the typically small lateral conductivity of organic semiconductor for some types of devices like OPVs and OLEDs. So, the concept of composite electrode is put forward. There are many methods to form a composite electrode with a silver nanowire, for example poly(3,4-ethylenedioxythiophene) polystyrene sulfonate (PEDOT:PSS) welding, graphene coating, double-layer structure, electrospun nanofibers, deposition of MnO2, TiO2, ZnO, AZO particles. The composite electrode can easily solve the problem of electrical conductivity and fill the gap between nanowires. Whereas PEDOT:PSS severely limits the device lifetime, and most of the nanoparticles need high temperatures (140 °C to 250 °C). Zilberberg et al. use sSnOx sol–gel process to fabricate the TEs even at room temperature with the method of atomic layer deposition (ALD).23 But ALD limits the roll-to-roll production. So, currently, it still cannot achieve a large scale of cost-effective production.10,15–23
Thirdly, AgNWs TEs are easily to fall off the substrate due to the poor adhesion, which limits both of its usage and mass production. The composite electrode is very helpful to improve adhesion. However, the current technology is not suitable for roll-to-roll production.
In this work, we report a solution method to fabricate AgNWs TEs on PET substrate at room temperature which is suitable to the roll-to-roll production. More importantly, the fabrication processes are scalable and cost effective. With this method, the Rsh of the TEs can be reduced by four orders while maintaining high transmission. In addition, the gaps between the nanowires are successfully filled and the adhesion between the AgNWs and the substrate are improved. Moreover, this flexible transparent electrode is applicable for any flexible substrate and ultimately for future wearable optoelectronic devices. This will be of great significance to the extension and application of the electrode.
To found the cause of the increase in conductivity, we analysed the solution. The solution of SnCl4·5H2O is not stable and easy to be hydrolysed. The reactions in the aqueous solution of SnCl4·5H2O can be expressed as:
SnCl4 + 6H2O → H2[Sn(OH)6] + 4HCl | (1) |
SnO2·6H2O + 6HCl → H2SnCl6 + 8H2O | (2) |
There are two main effects of SnCl4·H2O solution on TEs, which lead to the Rsh reduction of four orders in magnitude, from 90 kΩ sq−1 to 12 Ω sq−1.
Firstly, SnO2·xH2O can make the nanowire in close contact and fill the gap of AgNWs TEs. The nanowires will be adsorbed on the substrate due to the strong adhesion of SnO2 with substrate. And adhesion of SnO2 with glass can even reach 20 MPa. SnO2·xH2O can help the nanowires adhere firmly to the surface of the substrate and contact closely to each other for better transmission of electrons. Moreover, the filling of the voids by SnO2·xH2O is very important for electronic devices. The filling of the nonconductive voids can improve the collection of carriers which will improve the performance of electronic devices.
Secondly, Cl− ions could help to bind the AgNWs together and form a weld-like junction which will further increase the conductivity of the film. As discussed in previous studies,21 silver atoms in AgNWs may be dissolved slowly in the presence of Cl− and dissolved oxygen in water. Due to redox reactions, it will produce solvated silver ions (Ag+). The redox reaction can be written as:
4Ag + O2 +2H2O ↔ 4Ag+ + 4OH− | (3) |
We need to pay attention to the atomic oxygen on the silver surface. It may block the re-deposition of silver ions onto the silver surface. And atomic oxygen on the silver surface comes from molecular oxygen which is adsorbed and dissociated to atomic oxygen between 200 K and 500 K.24 However, concentration of dissolved oxygen in water is very limited so that Ag+ ions could redeposit onto the relatively more active AgNWs surface and junction. The deposition of Ag at the junction will allow the two nanowires to be successfully welded together and will reduce Rc, which is the main source of Rsh. So, the Cl− in the solution can help improve the conductivity of TEs.
In Table 1, the electrical properties of different composite TEs are compared and analysed. The last row presents our results, whose perform is seen to be better than other types of electrodes. When the length of the nanowire is doubled, the resistance is reduced by an order of magnitude. In contrast, while the diameter varies at 50–100 nm, the transmittance is maintained at 90%, the longer the nanowires are, the better the electrical properties. And we also found that when the length is the same, the thinner the nanowire is, the better the electrical properties are.
Composite TEs | Length (μm) | Diameter (nm) | Rsh (Ω sq−1) | Transmittance |
---|---|---|---|---|
AgNWs/PEDOT:PSS | 20–30 | 50–100 | 600 | 90% |
AgNWs/PEDOT:PSS | 50–100 | 50–100 | 54 | 90% |
AgNWs/RGO | 10–20 | 50–100 | 20 | 92% |
AgNWs/Aa-PDA | 10–20 | 40–50 | 20 | 94% |
AgNWs/sSnOx | 10–20 | 50–100 | 5.2 | 87% |
AgNWs/ZnO | 5–10 | 50–100 | 4.2 | 85% |
AgNWs/SnO2·H2O | 10–20 | 50–100 | 12 | 92% |
Fig. 3 Transmittance (T), scattering (S), and haze (H) properties of initial AgNWs TEs, SnO2·xH2O film and AgNWs/SnO2·xH2O composite TEs. |
As shown in Fig. 3, for the initial AgNW TEs (black line), fabricated by means of the doctor-blade coating method, the transmittance is over 92.9% (at 550 nm wavelength). But the Rsh is too high for the pure AgNW TEs. Similarly, the only SnO2·xH2O film (blue line) has a transmittance of 93% but its conductivity is not good enough yet. In contrast, for the composite TE, its transmittance is little changed and remained at 92.7%, but its conductivity is significantly improved, also its haze and scattering are increased by about 1%. This means that the presence of the SnO2·xH2O layer has little effect on the transmittance but will enhance the scattering due perhaps to the change of refractive index.
The junction of the composite TEs is tested by TEM to confirm the contact of the nanowires. Fig. 5a and b show the TEM images of the crossing structure of initial TEs and the composite TEs. For initial AgNWs TEs (Fig. 5a), the connection between the crossed AgNWs is not welded. And the force between the nanowires is mainly van der Waals force. For the AgNWs/SnO2·xH2O composite TEs, the connection between the crossed AgNWs is welded. The force of the weld-like junction is intermolecular force. Therefore, the nanowires are firmly and stably welded together although exfoliated by the ultrasonic from the substrate. This means that the solution of SnO2·xH2O can help to improve contact of nanowires.
Fig. 5 (a) TEM images of initial AgNWs crossing, (b) TEM images of weld-like AgNWs junction of AgNWs/SnO2·xH2O composite TEs. |
The elemental composition is determined by Energy Dispersive Spectrometer (EDS). Fig. 6c shows the EDS spectrum of the amorphous, and reveals the presence of tin (Sn), oxygen (O), carbon (C), copper (Cu) and chlorine (Cl) elements in the sample. Carbon is the most abundant. This could be attributed to the amorphous carbon-coated copper grids, which is also the source of copper. The small amount of chlorine comes from the H2SnCl6 in the solution. The most important thing is verifying the existence of tin and oxygen in the amorphous thought to be SnO2·xH2O. To further confirm our speculation, we need to remove the crystalline water from the amorphous to verify the existence of SnO2. When SnO2·xH2O is annealed at 400 °C for 30 min, SnO2·xH2O will be turned into the crystallized SnO2. The crystallized SnO2 is characterized by high resolution transmission electron microscopy (HRTEM). The HRTEM image shows a clear lattice spacing of 3.3 Å in Fig. 6b, which exactly matches to the (110) plane of single crystal SnO2.
Fig. 6d presents the XRD patterns of this crystalline substance. The major XRD peaks at 2θ = 26.61, 33.89, 37.95, 51.78 and 65.94° are assigned to the (110), (101), (200), (211) and (301) reflection planes of tetragonal SnO2, respectively. The diffraction peaks of the products can be well indexed to the known tetragonal rutile SnO2 (JCPDS 41-1445), which confirms the presence of SnO2 in the annealed products. So far, the amorphous material is determined to be SnO2·xH2O.
This simple heat treatment surprisingly gives us an unexpected benefit that the adhesion of the film is significantly improved. As we all know, the thin film of AgNWs can easily be erased when we touch it gently due to the poor adhesion of the initial AgNWs TEs. However, there's always a way out! The adhesion of the composite electrodes is improved significantly just with a 100 °C or 200 °C heating treatment. This is attributed to the strong adhesive strength between SnO2 and the substrate. When the non-heated composite electrodes were taped and torn down just for one time, the Rsh increased from 12 to 60 Ω sq−1 which is increased by 5 times (black line in Fig. 7b). Nevertheless, the 100 °C or 200 °C heating treatment has only a little influence on the conductivity of the composite TEs (Fig. 7b). The Rsh increases only by 3 Ω sq−1. In addition, the thermal stability of the heated composite electrode is quite good. The Rsh of the film changes little but maintains at about 12 Ω sq−1 during heating (Fig. 7c). In conclusion, the adhesion of the composite TEs can be improved by heat treatment, and the TEs can also tolerate adhesive tape test.
XPS spectra are used to characterize the initial composite TEs and the heated composite TEs at 200 °C. We want to know whether the heat treatment has other effects on the electrode, in addition to the loss of crystalline water. Fig. 8 shows the X-ray photoelectron spectroscopy (XPS) of the composite TEs. The XPS survey spectrum (Fig. 8a) shows the peaks of Ag 3d doublet, Sn 3d doublet, Sn 4d and O 1s peaks. There are two peaks with binding energies of 368.3 eV for Ag 3d5/2 and 374.3 eV for Ag 3d3/2 in the regional spectrum (Fig. 8b) of Ag 3d. This is consistent with the standard binding energy of pure silver. The peaks at a binding energy of 486.6, 495.3 and 27.1 eV (Fig. 8c) can agree with the Sn 3d5/2, Sn 3d3/2 and Sn 4d3/2, respectively. Their standard combination can be very close to the previously reported results, indicating that the valence states of Ag and Sn are 0 and +4, respectively. This means that the heat treatment at 200 °C does not cause a change in the valence of the composite electrode.
Fig. 8 XPS spectra of SnO2·xH2O. (a) General XPS spectra of initial and 200 °C heating SnO2·xH2O. (b) Ag 3d XPS spectrum of SnO2·xH2O. (c) Sn 3d XPS spectrum of SnO2·xH2O. |
This journal is © The Royal Society of Chemistry 2018 |