Elaheh Pousaneha,
Tobias Rüffera,
Khaybar Assima,
Volodymyr Dzhaganbc,
Julian Nolla,
Dietrich R. T. Zahnb,
Lutz Mertensd,
Michael Mehringd,
Stefan E. Schulzef and
Heinrich Lang*a
aTechnische Universität Chemnitz, Faculty of Natural Sciences, Institute of Chemistry, Inorganic Chemistry, D-09107 Chemnitz, Germany. E-mail: heinrich.lang@chemie.tu-chemnitz.de; Fax: +49-(0)371-531-21219; Tel: +49(0)371-531-21210
bTechnische Universität Chemnitz, Faculty of Natural Sciences, Institute of Physics, Semiconductor Physics, D-09107 Chemnitz, Germany
cV. E. Lashkaryov Institute of Semiconductors Physics, National Academy of Sciences of Ukraine, 03028 Kyiv, Ukraine
dTechnische Universität Chemnitz, Faculty of Natural Sciences, Institute of Chemistry, Coordination Chemistry, D-09107 Chemnitz, Germany
eTechnische Universität Chemnitz, Center for Microtechnologies, D-09107 Chemnitz, Germany
fFraunhofer Institute for Electronic Nano Systems ENAS, Technologie-Campus 3, D-09126 Chemnitz, Germany
First published on 29th May 2018
The synthesis and characterization of bis(ketoiminato)magnesium(II) complexes of composition [Mg(OCR2CH2CHR1NCH2CH2X)2] (X = NMe2: 3a, R1 = R2 = Me; 3b, R1 = Me, R2 = Ph. X = OMe: 3c, R1 = R2 = Me) are reported. Complexes 3a–c are accessible by the reaction of C(O)R2CH2CHR1N(H)CH2CH2X (X = NMe2: 1a, R1 = R2 = Me; 1b, R1 = Me, R2 = Ph. X = OMe: 1c, R1 = R2 = Me) with MgnBu2. The structure of 3b in the solid state was determined by a single crystal X-ray diffraction study, confirming that the Mg(II) ion is hexa-coordinated by two ketoiminato ligands, while each of the latter coordinates with its two N- and one O-donor atom in an octahedral MgN6O2 coordination environment in the OC-6-33 stereo-isomeric form. The thermal behavior of 3a–c was studied by TG and DSC under an atmosphere of Ar and O2 respectively. The respective Me-substituted complexes 3a,c decompose at lower temperatures (3a, 166 °C; 3c, 233 °C) than the phenyl derivative 3b (243 °C). PXRD studies indicate the formation of MgO. Additionally, TG-MS studies were exemplarily carried out for 3a, indicating the release of the ketoiminato ligands. Vapor pressure measurements were conducted at 80 °C, whereby 3a,c possess with 5.6 mbar (3a) and 2.0 mbar (3c) significantly higher volatilities than 3b (0.07 mbar). Complexes 3a–c were used as MOCVD precursors for the deposition of thin MgO films on silicon substrates. It was found that only with 3a,c thin, dense and rather granulated MgO layers of thicknesses between 28–147 nm were produced. The as-deposited MgO layers were characterized by SEM, EDX, and XPS measurements and the thicknesses of the as-deposited layers were measured by Ellipsometry and SEM cross-section images. Apart from magnesium and oxygen a carbon content between 3–4 mol% was determined.
Magnesium oxide films can be produced by different methodologies, including the sol–gel process,12,13 molecular beam epitaxy,14 pulsed-laser deposition,15 ion beam sputtering,16 electron beam evaporation,17 and laser ablation.18 For the formation of high-quality MgO deposits, CVD (Chemical Vapor Deposition) and ALD (Atomic Layer Deposition) are best suited, since uniform, conformal, and variable film thicknesses are obtained.19
Over the last few years, various organometallic and metal–organic compounds have been used as MgO CVD precursors, including [Mg(η5-C5H4R)2] (R = H,20 R = Me (ref. 21)), [Mg(β-diketonate)2] (β-diketonate = acac,22 thd22,23), [Mg(β-diketonate)2(tmeda)] (β-diketonate = thd,3,24 = hfac1), [Mg(O2CR)2] (R = C7H15, CNEt2),25 [Mg4Me4(OtBu)4],26 [Mg6(O2CNEt2)12],27 [Mg(DMADB)2]6, and [bis[5-N-(N,N-dimethylaminopropyl)-2,2,7-trimethyl-3-octanonato] magnesium]28 (acac = acetylacetonate, thd = 2,2,6,6-tetramethyl-3,5-heptanedionate, hfac = 1,1,1,5,5,5-hexafluoro-2,4-pentanedionate, tmeda = N,N,N′,N′-tetramethylethylenediamine, DMADB = N,N-dimethylaminodiboranate). Among them, the magnesium β-diketonates are very promising CVD precursors, due to their ability to fulfill the requirements needed for gas-phase deposition experiments, which are, for example, high stability and cost-effective and straightforward high yield synthetic methodologies.3,22
In order to avoid oligomerization processes, which may take place, for example, with β-diketonate or β-ketoiminate magnesium complexes, it is advantageous to introduce a third coordination site such as OR or NR2 units (R = single bonded organic group) at the respective chelating ligands.3 These groups are able to occupy an additional coordination site on the alkaline earth metals leading to less oligomerization of the molecules and thus increase the volatility of the complexes. In this respect, Rees and co-workers reported on the synthesis of the first example of such a metal–organic species, bis[5-N-(N,N-dimethylaminopropyl)-2,2,7-trimethyl-3-octanonato]magnesium,28 which successfully could be applied as precursor in the CVD process for MgO thin layer formation.28
This prompted us to enrich the family of β-ketoiminato magnesium complexes by three additional species, [Mg(OCR2CH2CHR1NCH2CH2X)2] (X = NMe2, OMe; R1, R2 = Me, Ph), in order to gain a better insight into the deposition performance of such type of complexes.
The 1H NMR spectra were performed with a Bruker Avance III 500 spectrometer operating at 500.3 MHz for 1H and at 125.8 MHz for 13C{1H} in the Fourier transform mode. The chemical shifts are reported in δ units (parts per million) relative to tetramethylsilane. Infrared spectra were recorded with a Thermo Nicolet IR 200 spectrometer. The melting points were determined with a Gallenkamp MFB 595 010 M melting point apparatus. High-resolution mass spectra were conducted with a micrOTOF-QII Bruker Daltonite workstation.
TGA/DSC experiments were performed with a Mettler Toledo TGA/DSC1 1100 system with a UMX1 balance. The TG-MS experiment was performed with a Mettler Toledo TGA/DSC1 1600 system with a MX1 balance coupled with a Pfeifer Vacuum MS Thermostar GSD 301 T2 mass spectrometer. For PXRD measurements the STOE powder diffractometer STOE Stadi P with Ge(111) monochromator Cu-Kα radiation (λ = 0.15406 nm, 40 kV, 40 mA) was applied. Chemical vapor deposition experiments were carried out in a home-built vertical cold-wall reactor equipped with a heater surface dimension of 20 × 20 mm from BACH Resistor Ceramics GmbH.29 A heat capacity measurement of up to 520 °C could be realized, controlled by a Gefran 600 module, which is connected with a Pt 100 thermo sensor. The carrier gas flow (N2, 50 mL min−1) and the reactive gas flow (O2, 40 mL min−1) were controlled by MKS type 247 mass flow controllers connected to the reactor by heated copper lines. The pressure within the reactor was controlled with an Edwards Active Gauge Controller (PKR 251). The continuous evaporation of the MOCVD precursors was carried out by an oil pump (EXC 120) from Edwards. The thickness of the layers was measured using Spectroscopic Ellipsometry M–2000UI from J. A. Woolam Co. (wavelength range 245–1690 nm (5.06–0.73 eV), angle of incidence 45, 50, 55, 60, 70, and 75°). The surface morphology of the as-prepared layers was investigated by field-emission scanning electron microscopy (SEM) using a ZEISS Supra 60 SEM microscope. Energy-dispersive X-ray analyses were carried out with a Bruker Quantax 400 system, attached to the SEM to determine the chemical composition of the films (operating voltage 3 keV). XPS measurements were performed with an ESCALAB 250Xi XPS Microprobe (Thermo Scientific) equipped with a monochromatized Al Kα X-ray source (hν = 1486.6 eV). The survey and high-resolution spectra were acquired at a bandpass energy of 200 and 20 eV, respectively. The binding energy was calibrated with respect to the C1s peak at 284.5 eV. Avantage (Thermo Scientific) software was used for XPS spectra analysis and the calculation of the atomic composition of the samples (Scofield relative sensitivity factors were applied30).
β-Ketoimines 1a,5 1b31 and 1c32 were prepared according to literature procedures by the condensation reaction of the appropriate β-diketones with one equivalent of the corresponding amine. The isolated β-ketoimines were dried with MgSO4 and purified via distillation under reduced pressure.
Mp. 130 °C. Anal. calcd. (%) for C18H34MgN4O2: C 59.59, H 9.45, N 15.44; found C 59.35, H 9.56, N 15.40. IR (KBr, v/cm−1): 2980 vw, 2920 vw, 1612 m, 1579 s, 1505 s, 1482 s, 1411 s, 1339 s, 1289 w, 1243 w, 1019 m, 930 m, 786 m, 786 m, 733 s, 668 m. 1H NMR (C6D6, δ): 1.63 (s, 6H, NCMe), 1.96 (s, 12H, NMe2), 1.98 (s, 6H, OCMe), 2.6–3.0 (m, 8H, N(CH2)2), 4.92 (s, 2H, CH). 13C{1H} NMR (C6D6, δ): 21.84 (NCMe), 27.91 (OCMe), 46.33 (NMe2), 46.61 (NCH2), 59.17 (NCH2), 95.89 (CH), 171.04 (CNMe), 180.90 (OCMe). HR-MS: calcd for C18H34MgN4O2: 362.2532; found m/z = 363.2617 [M + H]+.
Mp. 180 °C. Anal. calcd. (%) for C28H38MgN4O2: C 69.07, H 7.87, N 11.51; found C 68.54, H 7.90, N 11.29. IR (KBr, v/cm−1): 2990 vw, 2910 vw, 1588 s, 1500 s, 1420 s, 1477 s,1344 s, 1289 m, 1259 m, 1113 w, 1025 m, 1068 w, 942 w, 859 m, 796 m,782 m, 752 s, 712 s, 682 s. 1H NMR (C6D6, δ): 1.75 (s, 6H, NCMe), 1.95 (s, 12H, NMe2), 2.7–3.1 (m, 8H, N(CH2)2), 5.74 (s, 2H, CH), 7.08–8.14 (m, 10H, Ph), 13C {1H} NMR (C6D6, δ): 22.49 (NCMe), 45.43 (NCH2), 59.05 (NCH2), 46.82 (NMe2), 94.14 (CH), 127.39 CHCCO, 128.35 (CHCHC), 128.40 (CHCHCH), 143.30 (CHCCO), 171.69 (CNMe), 175.10 (OCPh). HR-MS: calcd. for C28H38MgN4O2: 486.2845; found m/z = 487.2953 [M + H]+.
Mp. 110 °C. Anal. calcd. (%) for C16H28MgN2O4: C 57.07, H 8.38, N 8.32; found C 56.77, H 8.65, N 8.27. IR (KBr, v/cm−1): 2990 vw, 2910 vw, 1582 s, 1504 s, 1478 s,1410 s, 1340 s, 1108 m, 1071 m, 1033 m, 1007 w, 936 m, 864 w, 736 m, 661 w. 1H NMR (C6D6, δ): 1.58 (s, 6H, NCMe), 2.02 (s, 6H, OCMe), 3.02 (s, 6H, OMe), 3.1–3.7 (m, 8H, N(CH2)2), 4.94 (s, 2H, (CH). 13C{1H} NMR (C6D6, δ): 21.53 (NCMe), 27.99 [OCMe), 48.21 (NCH2), 58.65 (OMe), 71.59 (NCH2), 96.46 (CH), 169.98 (CNMe), 181.63 (OCMe). HRMS: calcd. for C16H28MgN2O4: 336.1899; found m/z = 337.1985 [M + H]+.
a Rint = ∑|F02 − F02 (mean)|/∑F02, where F02 (mean) is the average intensity of symmetry equivalent diffractions.b S = [∑w (F02 − F20)2]/(n − p)1/2, where n = number of reflections, p = number of parameters.c R = [∑(‖F0| − |F0|)/∑|F0|); R[∑(w(F02 − F02))2/∑(wF04)]1/2. | |
---|---|
Compound | 3b |
Empirical formula | C28H38MgN4O2 |
Formula mass (g mol−1) | 486.93 |
Crystal system | Orthorhombic |
Space group | Pccn |
a (Å) | 10.3635(2) |
b (Å) | 16.8790(4) |
c (Å) | 15.2483(3) |
V (Å3) | 2667.32(10) |
Z | 4 |
Dcalc(Mg m−3) | 1.213 |
Wavelength (Å) | 1.54184 |
Temperature (K) | 120 |
Absorption coefficient (mm−1) | 0.818 |
F(000) | 1048 |
Reflections collected | 5165 |
Reflections unique/Rinta | 2303/0.0245 |
Goodness-of-fit on F2b | 1.025 |
Data/restrains/parameters | 2304/27/200 |
θ Range for data collection (°) | 5.008 to 65.981 |
Limiting indices | −12 ≤ h ≤ 11, −18 ≤ k ≤ 19, −10 ≤ l ≤ 17 |
Final R indices [I > 2σ(I)]c | R1 = 0.0448, wR2 = 0.1100 |
R Indices (all data)c | R1 = 0.0483, wR2 = 0.1124 |
Largest diff. peak/hole (e Å−3) | 0.241 and −0.263 |
(1) |
The identity of 3a–c has been confirmed by 1H, 13C{1H} NMR and IR spectroscopy, elemental analysis and high-resolution ESI-TOF (Electro Spray-Ionization Time-of-Flight) mass spectrometry. The structure of 3b in the solid state was determined by single crystal X-ray structure analysis. The thermal decomposition behavior of 3a–c was studied by TG and DSC measurements. In addition, the vapor pressures of these species were determined.
The 1H NMR spectra of 3a–c show the characteristic singlets for the respective ketoiminato CH protons at 4.92 (3a), 5.74 (3b) or 4.94 ppm (3c). As expected, these resonances are somewhat downfield shifted, when compared to the respective ketoimines 1a–c (1a, 4.87; 1b, 5.69; 1c, 4.86 ppm) and hence this shifting can be used to monitor the reaction to give 3. During the course of this reaction, the signal of the enolic oxygen-bonded hydrogen atom in 1a–c disappears. All other resonance signals are found as expected.
In the 13C{1H} NMR spectra, the CH carbon signals of the respective ketoiminato units are observed at 95.89 (3a), 94.14 (3b) or 96.46 ppm (3c), which is in accordance with spectra of other Mg-ketoiminato complexes.28 The NCMe carbons resonate at 21.84 (3a), 22.49 (3b) and 21.53 (3c) ppm. The respective signals are shifted to lower field as compared to the reactants 1a–c (18.47 (1a), 19.05 (1b) and 18.56 (1c)).
The IR spectra of 3a–c are characterized by strong ν(CN) vibrations at 1580–1590 cm−1. Compared to 1a–c these bands are shifted towards lower frequencies confirming the coordination of 1a–c to Mg(II).32
High-resolution ESI-TOF studies show the molecular ion peak [M + H]+ at m/z = 363.2617 for 3a, 487.2953 for 3b and 337.1985 for 3c.
The phenyl derivative 3c shows with 180 °C a significant higher melting point than the methyl-functionalized species 3a,b (130, 110 °C).
As shown in Fig. 1, the Mg(II) ion is hexa-coordinated by two tridentate β-ketoiminato ligands occupying meridional sides and a distorted octahedral MgN2O6 coordination geometry in the OC-6-33 form. Deviations from the idealized octahedral geometry are observed, for example, the bond angles of trans- and cis-bonded donor atoms range from 164.87(8) to 165.4(3)° and 76.8(3) to 104.2(8)°, respectively (Fig. 1). The Mg–N2 distance of 2.46(2) Å is larger than the Mg–N1 one (2.1266(13) Å), confirming an unsymmetrical distribution of the charge within the delocalized ketoiminato ligand, which is comparable with bis[5-N-(N,N-dimethylaminopropyl)-2,2,7-trimethyl-3-octanonato]magnesium.28
Fig. 2 TG traces of 3a–c under an atmosphere of argon (left) and O2 (right) (gas flow 20 mL min−1, heating rate 10 °C min−1). |
Compd. | Onset temp. Ar [°C] | Onset temp. O2 [°C] |
---|---|---|
a Ar, O2 (gas flow 20 mL min−1) (Ar carrier gas flow 40 mL min−1, heating rate 10 °C min−1). | ||
3a | 152 | 166 |
3b | 253 | 243 |
3c | 120 | 233 |
The appropriate TG traces obtained under an atmosphere of argon show that the thermal decomposition of 3a,c occurs in two steps, while 3b shows only a single step decomposition (Fig. 2). The nature of the β-ketoiminato ligands has a significant effect on the decomposition temperature of 3a–c. This was observed, for example, for the phenyl containing β-ketoiminate as the respective complex 3b exhibits the highest thermal stability (Table 2). In contrast, complex 3c shows the lowest onset temperature of 120 °C in the argon atmosphere. A similar behavior was observed by Podkościelna et al.34 in the course of thermal behaviors study of copolymers naphthalene-2,7-diol dimethacrylate derivatives, which highest thermal stability was obtained in presence of aromatic rings.34
A different thermal behavior was observed for 3a–c, when the experiments were carried out under oxygen (Fig. 2). In contrast to the studies under argon, the complexes 3a–c follow a multi-step decomposition under oxygen. This is probably due to the reactivity of oxygen, which could produce during the heating process MgCO3 and additional C,O fragments,35,36 and lead to multiple thermal decomposition processes.
In terms of the residues obtained from the TG experiments, 3a showed with 8.9% (O2) and 10.5% (Ar) lower values than calculated for MgO (11.0%), demonstrating that this complex partially evaporates during the heating process. For 3b,c the weight of the residues are somewhat higher than the theoretical values (3b, O2: 9.2%, Ar: 8.6% (theory 8.2%). 3c, O2: 15.9%, Ar: 12.1% (theory 11.8%)). This indicates that most probably the respective residues contain some impurities.
The DSC traces of 3a–c under O2 are shown in Fig. 3, while those under Ar are depicted in the ESI (Fig. S1–S3†). The appropriate DSC traces are characterized by endothermic and exothermic processes. The endothermic peak at 180 °C (3b), which appears only under argon, confirms the melting of this complex (Fig. S2, ESI†). Under an atmosphere of oxygen, however, characteristic exothermic peaks are observed at 243 °C (E = 178.02 J g−1) (3a), 491 °C (E = 3649.47 J g−1) (3b) and 445 °C (E = 1447.26 J g−1) (3c), belonging to the decomposition of the respective complexes (Fig. 3).
Fig. 3 DSC traces of 3a–c under oxygen (oxygen carrier gas flow 20 mL min−1, heating rate 10 °C min−1). |
PXRD measurements of the residues of the TG experiments confirmed the formation of crystalline MgO (ICDD 01-071-1176). Representative, the diffractogram of 3a is depicted in Fig. 4, whereas those of 3b and 3c can be found in the ESI (Fig. S4–S5†). The related crystallite sizes were calculated by using the Scherrer equation based on reflection (200). The evaluation displays crystallite sizes of 15 ± 1 (Ar) and 17 ± 1 nm (O2) for 3a, while values between 8–17 nm were calculated for 3b and 3c (see captions of Fig. S4 and S5†).
Fig. 4 PXRD pattern of the TG residues of 3a under argon (top) vs. under oxygen (middle); red: crystalline MgO (ICDD 01-071-1176). (Crystal size: top: 15 ± 1 nm, middle: 17 ± 1 nm). |
On the example of 3a, TG-MS-coupled experiments were performed in order to obtain a deeper insight into the decomposition behaviour of 3a–c. The appropriate TG-MS traces, including the TG and the ion current curves of the respective mass-to-charge ratios (m/z) are depicted in Fig. 5. The mass-loss can be described as a partial evaporation and decomposition of 3a. Within this study we were not able to detect either the molecular ion peak, nor the β-ketoiminato ligand Me2N(CH2)2NCMeCHCMeO+, rather fragments such as m/z = 15 (CH3+), 29 (C2H5+, CHO+), 44 (C3H8N+, C3H6O+) and 58 (CH3CHO+), corresponding to the chelating β-ketoiminato unit.
The vapor pressures of the selected magnesium oxide precursors are summarized in Table 4. As it can be seen from this table, 3a (5.6 mbar at 80 °C) and 3c (2.0 mbar at 80 °C) possess higher values than reported magnesium precursors, i.e. [Mg(tfac)2(tmeda)] (0.46 mbar at 93 °C), [Mg2(thd)4] (0.2 mbar at 120–130 °C), [Mg(thd)2(tmeda)] (0.2 mbar at 100–110 °C), Mg(thd)2(dien)] (1.20 mbar at 110–130 °C) and [Mg(thd)2(trien)] (0.30 mbar at 145–170 °C). In comparison, the vapor pressure of 3b (0.07 mbar at 80 °C) is in the same order of magnitude.38,39 However, since the methodologies used to determine vapor pressures are quite different, the comparison of the vapor pressure values might be misleading in some cases.
Complex | Vapor pressure [mbar] | At temperature [°C] | Literature |
---|---|---|---|
a tfac = 1,1,1-trifluoropentan-2,4-dionate, tmeda = N,N,N′,N′-tetramethylethylenediamine, deeda = N,N′-diethylethylenediamine, dien = diethylenetriamine, trien = triethylenetetraamine. | |||
3a | 5.6 | 80 | — |
3b | 0.07 | 80 | — |
3c | 2.0 | 80 | — |
[Mg(thd)2(trien)] | 0.30 | 145–170 | 38 |
[Mg2(thd)4] | 0.2 | 120–130 | 38 |
[Mg(thd)2(tmeda)] | 0.2 | 100–110 | 38 |
[Mg(thd)2(deeda)] | 0.21 | 90–100 | 38 |
[Mg(thd)2(dien)] | 1.20 | 110–130 | 38 |
[Mg(tfac)2(tmeda)] | 0.46 | 93 | 39 |
The respective precursors were heated to temperatures between 80–120 °C in the vaporizer unit of the CVD reactor under reduced pressure. The reactor glass cover was additionally heated to approximately 100 °C. These measures were necessary to achieve a convenient precursor flow rate. The deposition time was set to 60 min for all precursors in order to have uniform conditions. According to the TG studies the substrate temperature was set to 450 °C for complexes 3a–c and additionally to 510 °C for 3b. The applied deposition conditions are summarized in Table 5. As result thereof, it can be rated that 3a,c gave MgO layers, while 3b did not result in magnesium oxide film formation up to 510 °C. This is most probably attributed to the higher decomposition temperature and hence higher thermal stability of this complex as investigated by TG and DSC studies. The as-deposited films are of thicknesses between 28 and 147 nm, evidenced from the cross-sectional images shown below. The thinner films are beige coloured, whereas thicker films possess a dark blue appearance.
Compd. | θ(dep.) [°C] | θ(Precursor) [°C] | Thicknessc [nm] | Pressure [mbar] | N2 flow rate [mL min−1] | O2 flow rate [mL min−1] | Growth rate [nm min−1] |
---|---|---|---|---|---|---|---|
a In presence of oxygen.b Without addition of oxygen.c Determined from Ellipsometry. | |||||||
3aa | 450 | 80 | 28.3 | 1 | 50 | 40 | 0.47 |
3ab | 450 | 80 | 69.6 | 1 | 50 | — | 1.16 |
3ba | 450, 510 | 120 | — | 1 | 50 | 40 | — |
3bb | 450, 510 | 120 | — | 1 | 50 | — | — |
3ca | 450 | 90 | 44.6 | 1 | 50 | 40 | 0.74 |
3cb | 450 | 90 | 147.0 | 1 | 50 | — | 2.45 |
Fig. 7 SEM images of the as-deposited films (applied parameters are given in Table 5). Films A and C were obtained, when the depositions were carried out under oxygen (N2/O2 ratio 10/8). Films B and D without oxygen. Images A, B: deposits from 3a; C, D: from 3c. |
The film thicknesses were determined by cross-section SEM images (Fig. 8) and Ellipsometry (Table 5). Utilizing the layer thicknesses obtained by Ellipsometry, the growth rate per minute was calculated for each precursor (Table 5). Thereby, metal–organic complex 3c possesses with 2.45 nm min−1 the highest growth rate. As it can be seen from Fig. 8 and from Fig. S6–S8 (ESI†), the films formed without addition of any reactive gas are thicker (3a, 69.6 nm; 3c, 147.0 nm), if compared to those obtained from the experiments with oxygen (3a, 28.3 nm; 3c, 44.6 nm). This is most probably based on reactions of the precursors with oxygen in gas phase yielding less precursor molecules on the substrate surface. The thicknesses of the MgO layers determined by cross-section SEM images show slightly different values with Ellipsometry (3a, 63 nm; 3c, 135 nm (Ar) and (3a, 29 nm; 3c, 43 nm (O2)).
Fig. 8 Cross-section image of the MgO layer obtained from 3a, substrate temperature 450 °C, deposition time 1 h, working pressure 1 mbar, N2 (50 mL min−1). |
The as-deposited layers were analyzed by EDX (3a, (O2) Fig. 9 and layers 3a (N2) and 3c, Fig. S9–S11 (ESI†)). From the EDX spectra of 3a,c peaks for Mg, O, N, C, and Si can be seen of which O (partly) and Si can be assigned to the substrate material (Fig. 9). Hence, the energy of the electron beam was reduced from 15 to 3 keV in order to reduce the penetration depth. As a result, thereof, the signals for the latter two elements decreased, while the respective signals for Mg increased (ESI, Fig. S9–S11†).
Fig. 9 EDX spectra of the as-obtained MgO film of 3a, N2 (50 mL min−1), O2 (40 mL min−1), substrate temperature 450 °C. |
Additionally, XPS measurements were performed on the obtained MgO films. For removing surface contaminations, the layers were preliminary sputtered with argon ions with energies of 4.0 keV for 2 min. A typical XPS spectrum of a MgO layer deposited at 450 °C using 3c as precursor is shown in Fig. 10. The XPS spectra of all other samples are presented in the ESI (Fig. S12–S14†) and the related XPS results are summarized in Table 6. The peaks arising from Mg 2p, O 1s, C 1s, and Si 2s appear at 50.6, 531.0, 284.2 eV, and 153.6 eV, respectively, and were used to calculate the chemical composition of the layers. The position of the Mg 2p (BE = 50 eV), as well as of Mg 1s (BE = 1303 eV), Mg 2s (89 eV) and O1s (530.5 eV) peaks are in good agreement with the earlier reports on MgO,40,41 confirming the MgO as the main phase. This could be also verified by the oxygen content of the samples. For the two thinner films, 28 and 44 nm, oxygen from the substrate distorts the Mg:O ratio in the latter two samples, but the two thicker films without substrate contribution show Mg:O ratio close to 1:1 (Table 6). The high-resolution XPS spectra reveal relatively sharp and symmetrical Mg 2p and O 1s in the sputtered sample (ESI, Fig. S15†), while in the as-deposited one additional contributions of hydroxide species at higher BEs contribute to both spectra, as commonly observed for MgO surface.41 Si peaks appear after sputtering, most probably partially originating from the Si/SiO2 substrate surface.
Fig. 10 XPS spectra of the MgO film obtained from 3a at 450 °C (N2, 50 mL min−1; after 2 min sputtering, Ar+, 4.0 keV). |
Complexes 3a,c produced MgO layers, which show less carbon contamination (3–4%) in comparison to similar molecules such as ketoiminate [bis[5-N-(N,N-dimethylaminopropyl)-2,2,7-trimethyl-3-octanonato]magnesium] (7% carbon content after 120 min sputtering).28 The studies confirm the suitability of the 3a,c precursors for the formation of MgO layers by the MOCVD process.
To evaluate the crystallinity of the as-deposited films, PXRD measurements were performed for all samples obtained from the CVD studies. Thereby, the layer formed by using 3c without oxygen was the only sample that led to an assignable diffractogram (Fig. S16†). All other deposits did not reveal any reflexes indicating the amorphous nature of them. However, this could be also attributed to the film thickness as only the layer with 147 nm (3c) provided valuable data. From Fig. S16† it can be seen that the crystalline part of the film consists of cubic MgO (ICDD 01-071-1176).
Footnote |
† Electronic supplementary information (ESI) available: CCDC 1569233. For ESI and crystallographic data in CIF or other electronic format see DOI: 10.1039/c8ra01851k |
This journal is © The Royal Society of Chemistry 2018 |