Keumyoung Seo,
Taekyung Lim,
Sang-Mi Jeong and
Sanghyun Ju*
Department of Physics, Kyonggi University, Suwon, Gyeonggi-Do 443-760, Republic of Korea. E-mail: shju@kgu.ac.kr
First published on 22nd May 2018
In this study, we investigated the reduction of a 3D microporous NiOx structure, used as a metal oxide catalyst, by proton irradiation with polyvinylpyrrolidone (PVP) for hydrogen regeneration. In general, the reduction process for hydrogen regeneration requires high temperatures (1000–4000 °C) to release saturated oxygen from the metal oxide catalyst. Proton irradiation with PVP could regenerate abundant oxygen vacancies by releasing the oxygen attached to NiOx at room temperature. The 3D microporous NiOx structure provided the maximum hydrogen generation rate of ∼4.2 μmol min−1 g−1 with the total amount of generated hydrogen being ∼460 μmol g−1 even in the repetitive thermochemical cycle; these results are similar to the initial hydrogen generation data. Therefore, continuous regeneration of hydrogen from the oxygen-reduced 3D microporous NiOx structure was possible. It is expected that the high thermal energy, which is the major problem associated with hydrogen regeneration through the conventional heat treatment method, would be resolved in future using such a method.
One of the representative environment-friendly hydrogen generation methods in the current stage of technological advancement is the water splitting method using alternative energy sources (solar, wind, and the latent heat of a power plant), based on photocatalysts, photosynthesis and microorganisms, and low-temperature thermochemical cycles.2 Among these methods, is the water splitting method based on a low-temperature thermochemical cycle, in which redox-accessible medium materials in a closed cycle configuration decompose water at a temperature of 1000 °C or less through a multiple-step chemical reaction. Theoretically, such a method can achieve a thermal efficiency of 80% or more, and has the advantage of using thermal energy sources like solar energy and the latent heat of a power plant.3,4 Since the first study on thermochemical water splitting conducted by Funk and Reinstrom in 1964, over 200 water decomposition thermochemical cycles have been proposed thus far. However, for a simple two-step thermochemical cycle, the use of the water-splitting method is limited when the redox reaction of the medium occurs at a reaction temperature as low as 1000 °C or less.5 Therefore, it is necessary to study the methods in which metal oxides are reduced using a lower energy because the reduction energy required for reduction of a metal oxide for hydrogen regeneration is higher than the oxidation energy required for hydrogen generation. Although studies on various metal oxide reduction methods are in progress, further research is required on metal oxide reduction methods that use lower energy.6
In this study, repeated regeneration of hydrogen on a 3D microporous NiOx structure with large specific surface area used as a metal oxide catalyst was carried out by proton irradiation with polyvinylpyrrolidone (PVP). After coating the PVP as a reduction catalyst onto the oxidized NiOx after hydrogen generation, the oxygen-rich NiOx could be effectively reduced by using the proton irradiation method. In addition, the changes in the pore size, specific surface area, and residual oxygen content of the 3D microporous NiOx structures were investigated before and after hydrogen generation as well as after proton irradiation with PVP.
Fig. 2(a) shows a comparison between the amounts of regenerated hydrogen obtained by applying two hydrogen regeneration methods, proton irradiation only and proton irradiation with PVP, with respect to the initial hydrogen generation. The temperature required for hydrogen generation was 800 °C. For NiOx reduced by only proton irradiation without using PVP as a reducing catalyst during hydrogen regeneration, the maximum hydrogen generation rate was ∼2.2 μmol min−1 g−1, and the total amount of generated hydrogen was ∼300 μmol g−1. On the other hand, in the case of NiOx reduced by proton irradiation with PVP, the maximum hydrogen generation rate was ∼4.2 μmol min−1 g−1, and the total amount of generated hydrogen was ∼460 μmol g−1, which were nearly the same as that obtained in the initial hydrogen generation. Note that the maximum hydrogen generation rate and amounts of hydrogen generated from previously reported metal oxide materials (FeAl2O4, CeO2, Ce0.75Zr0.25O2, and Co0.4Fe0.6Al2O4) were ∼3.6–33 μmol min−1 g−1 and ∼16.4–102 μmol min−1, respectively, at 1000–1350 °C.10–12 These reported values are comparable or lower than the results presented here. Typically, ion beam irradiation of an organic material can result in highly reactive free radicals by homolytic dissociation reactions, because organic materials are ionized and excited by the kinetic energy lost by ions colliding with the target materials.13–15 The determined activation energy of the 3D microporous NiOx structure was ∼1456 kJ mol−1. The proton irradiation method with PVP proposed in this study induces dissociation reaction of PVP by the physical and chemical energy of the protons to generate free radicals. Since the reduction of NiOx is promoted by highly reactive free radicals, the reduction efficiency of NiOx with PVP is higher than that of NiOx without PVP, resulting in an increase in hydrogen generation.
Fig. 2(b) shows the hydrogen generation and hydrogen regeneration characteristics of the 3D microporous NiOx structure. At 800 °C, the surface of the 3D microporous NiOx structure reacted with water vapor and oxidized, and hydrogen generation rapidly increased to a maximum within the initial 20 min. As the oxidation gradually becomes saturated, the hydrogen generation decreased to ∼40% of the maximum after ∼250 min. In the repetitive hydrogen regeneration experiment, the rate was similar to the initial maximum rate of ∼4.2 μmol min−1 g−1. Fig. 2(c) shows the degradation rates (C/C0) for hydrogen generation during repetitive redox cycles by proton irradiation of the 3D microporous NiOx structure, where C0 refers to the maximum amount of hydrogen and C refers to the amount of hydrogen at a certain time. As shown in Fig. 2(c), a similar C/C0 value during hydrogen regeneration confirms that the reduction method of proton irradiation with PVP for hydrogen regeneration is stable.
Typically, in the case of thermochemical cycles with metal oxide catalysts, the amount of Ni to be oxidized is proportional to the amount of hydrogen generated, as water splitting occurs during the conversion of metal into metal oxide. To identify the ratio of NiOx produced by the reaction of Ni and H2O vapor, TGA was performed on the samples after initial hydrogen generation as well as on samples undergoing redox reaction after proton irradiation with PVP (hydrogen regeneration). As seen in Fig. 2(d), for the pristine samples before the initial hydrogen generation, the oxidation of Ni to NiOx began at approximately 500 °C, and about 0.10, 0.47, and 1.35% NiOx (wt%) of were produced at approximately 600, 700, and 800 °C, respectively. Furthermore, the samples reduced by proton irradiation with PVP began to oxidize Ni at temperatures slightly higher than 500 °C with approximately 0.06, 0.34, and 1.42% NiOx (wt%) produced at about 600, 700, and 800 °C, respectively. On the other hand, oxidation of Ni in the proton irradiation only samples began at approximately 600 °C, with about 0.02, 0.15, and 0.60% NiOx (wt%) produced at approximately 600, 700, and 800 °C, respectively. A comparison of the amounts of NiOx confirms that complete conversion occurs in the sample subjected to redox reaction by proton irradiation with PVP after hydrogen generation. On the other hand, ∼50% conversion was observed for the sample proton irradiated without PVP. The conversion rates of hydrogen generation with PVP or without PVP are consistent with the amounts of generated hydrogen, as evident in Fig. 3(a). The proton irradiation method used for the reduction process reduces the oxygen-rich Ni surface and increases the amount of oxygen vacancies ( and , respectively) on the NiOx surface, further reacting with H2O vapor to produce hydrogen by the hydrogen generation process. Typically, metal oxide-based thermochemical cycles require high thermal energy through direct heating or concentration of sunlight to regenerate the oxygen vacancies in the metal oxide materials.7,16,17 However, the proton irradiation reduction method for the oxidized metal oxide has the advantage of room-temperature processing instead of a high temperature condition.
Fig. 3 (a) FE-SEM images, (b) BET surface area plots, and (c) XRD profiles of the same 3D microporous NiOx structure before and after hydrogen generation, and after proton irradiation with PVP. |
Fig. 3(a) shows the representative FE-SEM images of the 3D microporous NiOx structure before and after hydrogen generation, and after proton irradiation with PVP. The pore size and thickness of the 3D microporous NiOx structures used for hydrogen generation were ∼230 μm and ∼1.6 mm, respectively. As shown in Fig. 3(a), no change was observed in the surface structure of the 3D microporous NiOx structure, which is composed of 3D multi-pore structures. The most important factor that can increase the hydrogen generation efficiency of the hydrogen generation system using the metal oxide is the reaction surface area between the metal oxide material and H2O. To enlarge the reaction surface area, a nanoporous structure or nanoparticles are created by surface treatment of the metal oxide material to enhance the reactivity.18–21 However, these structures aggregate with each other as the hydrogen generation reaction proceeds, thereby reducing the reaction surface area and inhibiting the gas flow, consequently lowering the reaction rate. The 3D microporous NiOx structure proposed in this study is advantageous in that the structure can maintain its shape during the hydrogen generation and regeneration processes because it is composed of a 3D wire mesh structure.
The changes in surface area of the 3D microporous NiOx structure by thermochemical water splitting reaction during hydrogen generation were confirmed through the BET method. Fig. 3(b) shows the BET surface area plot of the 3D microporous NiOx structure before and after hydrogen generation, and after proton irradiation with PVP, respectively. The measured BET areas in all the three states confirmed that the surface areas were constant at 0.79 (before hydrogen generation), 0.73 (after hydrogen generation), and 0.75 m2 g−1 (after proton irradiation with PVP). This result indicates that the surface area of the 3D microporous NiOx structure is not critically affected by the repetitive process of hydrogen generation and proton irradiation with PVP.
Fig. 3(c) shows the XRD profiles of the 3D microporous NiOx structure before and after hydrogen generation, and after proton irradiation with PVP. For all the three conditions, three strong diffraction peaks (2θ) appearing at 44.5°, 51.8°, and 76.1° were ascribed to the (111), (200), and (220) planes of the 3D microporous Ni structure, respectively (ICDD PDF Card 87-0712, JCPDS. 2001). Five weak Bragg peaks (2θ) were observed at 37.4°, 43.4°, 62.9°, 75.4°, and 79.4°, which corresponded to the (111), (200), (220), (311), and (222) crystal planes (“Bunsenite” phase) of cubic NiO (JCPDS card No. 73-1523), respectively.22–24 The changes in the main diffraction peaks for the three conditions showed that the crystal peaks of the cubic NiO increased in intensity after hydrogen generation, while the corresponding NiO peaks decreased in intensity after proton irradiation with PVP. These results indicate that NiO was oxidized by reacting with H2O molecules according to the hydrogen generation process, and that it was effectively reduced after proton irradiation with PVP.
XPS analysis confirmed the chemical composition and chemical states of the outermost layer on the surface of the 3D microporous NiOx structure. Fig. 4 shows the XPS spectra of Ni 2p3/2 and O 1s before and after hydrogen generation, and after proton irradiation with PVP. As shown in Fig. 4(a) and (d), the XPS spectra for each condition showed Ni2+ and Ni3+ peaks related to the three oxidation states, NiO (854.0 eV for Ni 2p3/2, 529.1 eV for O 1s), Ni(OH)2 (855.6 eV for Ni 2p3/2, 530.6 eV for O 1s), and NiOOH (857.1 eV for Ni 2p3/2, 530.6 and 531.7 eV for O 1s).25–29 Typically, Ni(OH)2 and NiOOH peaks are formed by exposure to ambient humidity or by absorption of oxygen.30 Furthermore, the broad peak at ∼861 eV for Ni 2p3/2 is related to a “shake-up” satellite due to Ni 3d → Ni 4s transition, which is known to occur by excitation to higher energy levels through interactions between the valence electrons and outgoing electrons.31,32 The changes in oxidation before and after hydrogen generation and after proton irradiation with PVP were identified by calculating the ratio of Ni(OH)2 (855.6 eV) and NiOOH (857.1 eV) peak areas to the NiO (854.0 eV) peak area in Ni 2p3/2 and O 1s states. NiO was oxidized into Ni(OH)2 and NiOOH, and the (Ni(OH)2 and NiOOH)/NiO peak area increased from ∼1.29 (Ni 2p3/2)/∼0.84 (O 1s) to ∼1.47 (Ni 2p3/2)/∼2.10 (O 1s), respectively. However, the peak area decreased to 1.27 (Ni 2p3/2) and ∼0.78 (O 1s) due to the reduction effect after proton irradiation with PVP.
Fig. 4 XPS spectra of the 3D microporous NiOx structure before and after hydrogen generation, and after proton irradiation with PVP: (a–c) Ni 2p3/2 and (d–f) O 1s regions. |
This journal is © The Royal Society of Chemistry 2018 |