Ling Zhua,
Nan Zhaoab,
Lihong Tonga and
Yizhong Lv*a
aCollege of Resources and Environmental Sciences, China Agricultural University, Beijing 100193, China. E-mail: lyz@cau.edu.cn
bGuangdong Provincial Key Lab of Environmental Pollution Control and Remediation Technology, School of Environmental Science and Engineering, Sun Yat-sen University, Guangzhou 510275, China
First published on 7th June 2018
Potassium carbonate activated biochar (450 °C, 600 °C and 750 °C) and nonactivated biochar (600 °C) were prepared by using corn stalk as the raw material. These biochar samples were labeled as KBC450, KBC600, KBC750 and BC600. The physical and chemical properties of the biochar were strongly influenced by the activation of potassium carbonate. After activation with potassium carbonate, the aromatic, hydrophobic and non-polar properties of the biochar were enhanced to form an aromatized non-polar surface, and the aromatic properties were enhanced with the increase of the pyrolysis temperature. The outside surface of the activated biochar was similar to that of porous sponge with a mesoporous–microporous composite structure inside. The specific surface area of KBC600 was 5 times that of BC600, and KBC750 had a maximum surface area of 815 m2 g−1. Batch adsorption experiments showed that the adsorption capacity of KBC for naphthalene increased with the increase of pyrolysis temperature. The adsorption capacity of the biochar for naphthalene showed a significant positive correlation with O/C and (O + N)/C. KBC750 with the strongest surface hydrophobicity and the largest specific surface area had the largest adsorption capacity of 130.7 mg g−1. Physical adsorption and π–π EDA were the main adsorption mechanisms.
Due to the improvement of pore structure and surface chemical property, activated biochar usually has better adsorption capacity. It is believed that the increase of micropores will increase the adsorption capacity of biochar. Microporosity of H2SO4 activated biochar derived by pork bones increased by 263%, and the maximum adsorption capacity of methylene blue reached 61.3 mg g−1, which was nearly 3 times of that of unactivated biochar.10 It is noteworthy that many studies have shown that mesopores seem to be more suitable for adsorption of organic pollutants. In the study of the relationship between pore development and biochar adsorption properties, it was found that the adsorption capacity was mainly determined by biochar mesopores (1.7–50 nm) rather than its total area, and most micropores in biochar were not accessible to most nanoscale organic molecules.11 Not all activators enhance the specific surface area of biochar. Some of these activators mainly change the surface chemical properties of biochar, such as surface functional group composition and surface aromaticity. Surface chemical property is also one of the important properties that determine the biochar adsorption capacity. Activators have a significant effect on the surface chemical property of biochar. After HCl and HF elution, the carbon content, hydrophobicity and the aromatic functional group content were increased, while the polarity aliphatic chain char and hydroxyl were decreased, and these changes improved the adsorption of 2,4-D on biochar.12 Compared with acid-modified BC, alkali treatment would result in a larger surface area with higher surface aromaticity ratio (H/C) and higher N/C ratio with lower O/C values.13 Organic solvents also affect the surface properties of biochar. Since the changes of oxygen-containing functional group changed the interaction of π–π electron-donor–acceptor between modified biochar and tetracycline, the methanol-modified biochar increased the adsorption capacity of tetracycline by 45.6% compared with the primary biochar.14,15
Many studies have been conducted on the use of KOH as activator to activate biochar. The activation of KOH is mainly reflected in the increase of the number of mesoporous and specific surface area. Compared with physical activation, chemical activation using KOH usually results in a larger specific surface area with pores concentrated in a smaller pore size range. The increase of specific surface area makes the biochar activated by KOH have larger adsorption capacity. After activation by KOH, the mesoporous amount of potato straw biochar increased and the adsorption capacity of ciprofloxacin was enlarged.16 After activated by KOH, the specific surface area of municipal solid waste biochar increased by 64%, and the removal rate of methylene blue reached 99%.17 Actually, K2CO3 was formed in the activation process of KOH. The hydrolysis of K2CO3 can also produce KOH, and compared to KOH, K2CO3 is less corrosive, safer to use and easier to store. K2CO3 is a potential activator, but the effects of K2CO3 on the surface properties and adsorption behaviors of biochar were rarely reported. Meanwhile, in previous studies, biochar was immersed in activator solution. There are few studies on the preparation of activated biochar by directly impregnating biomass with activator solution. Therefore, K2CO3 was selected as activator in this study, and the straw is immersed in K2CO3 solution directly. Scanning electron microscopy, specific surface area and pore size distribution, infrared spectra were used for determining the structural characteristics and functional groups of biochars. The purpose of the study was to investigate the changes of surface characteristics for biochar after being activated by K2CO3, and naphthalene was used as adsorbate to study the adsorption characteristics and mechanism of biochar on non-polar pollutants.
The data obtained by the isothermal adsorption experiment were fitted with the Langmuir model (eqn (1)) and the Freundlich model (eqn (2)), respectively.
(1) |
Freundlich: qe = kfCe1/n | (2) |
Sample | Element content% | Atomic ratio | Yield% | Ash% | pH | |||||
---|---|---|---|---|---|---|---|---|---|---|
C | H | N | O | H/C | O/C | (O + N)/C | ||||
a O% = 100%-C%-H%-N%-ash%, the ash contains a small amount of P, S. | ||||||||||
KBC450 | 79.88 | 3.42 | 1.07 | 13.53 | 0.51 | 0.13 | 0.14 | 35.0 | 2.10 | 3.37 |
KBC600 | 80.79 | 2.42 | 0.89 | 13.79 | 0.36 | 0.13 | 0.14 | 31.8 | 2.11 | 3.53 |
KBC750 | 88.90 | 1.39 | 1.19 | 7.09 | 0.18 | 0.06 | 0.07 | 30.2 | 1.43 | 3.88 |
BC600 | 73.83 | 2.77 | 2.55 | 16.76 | 0.45 | 0.17 | 0.20 | 45.8 | 4.10 | 4.33 |
The carbon and hydrogen content of KBC increased with the temperature rising. At 600 °C, the carbon content of BC600 was lower than KBC600 and exhibited a higher hydrogen content, which indicated that potassium carbonate could promote the carbonation reaction and accelerate the dehydrogenation. With increasing temperature, the oxygen and nitrogen contents of KBC showed no regular changes but all lower than BC600, indicating that the addition of potassium carbonate made nitrogen and oxygen more easily lost. The atomic ratio could be used to characterize the aromaticity, hydrophobicity, and polarity of biochar. With the increase of O/C, (O + N)/C and H/C, the hydrophilicity and polarity increased while aromaticity decreased.20 The hydrophobicity and nonpolarity of BC600 were less than KBC, and the aromaticity was less than KBC600 and KBC750. The aromaticity of KBC450 was smaller than that of BC600, which might be caused by the lower pyrolysis temperature. The difference between BC600 and KBC showed that the addition of potassium carbonate during the preparation could change the pyrolysis process of biomass. H/C of KBC decreased with the increasing pyrolysis temperature. O/C, (O + N)/C of KBC450 and KBC600 did not change with the temperature increasing, while KBC750 was decreased. Therefore, the hydrophobicity and nonpolarity of KBC450 and KBC600 did not change significantly with the increase of temperature, and the hydrophobicity and nonpolarity of KBC750 were enhanced. Zhang et al. (2016) have shown that the addition of potassium carbonate and the formation of potassium hydroxide during the impregnation process would destroy the cellulose structure, weaken the hydrogen bonds between the cellulose molecules, and reduce the activation energy of the reaction, so that the pyrolysis of high polymer molecules in a high temperature conditions were more thorough.21 Nishimura et al. (2009) showed that K+ reacted with the glycosidic linkages of the cellulose polysaccharide units under high temperature conditions and changed the cellulose structure under the combined action of carbon dioxide. Compared with the classical levoglucosan structure,22 the final structure was a ring-opening polyhydroxy structure and forms O−K+ structure.23 Under these structural conditions, the addition and polycondensation reaction would be easier, and the polarity and hydrophilicity would be decreased. Under acid conditions, K+ will be replaced by H+, which was one of the reasons why the acidity of KBC was stronger than BC600.
Fig. 1 SEM images of KBC/BC600 (a, b, c, d expressed KBC450, KBC600, KBC750, BC600 respectively. Red arrows indicate non-penetrating pits). |
It could be speculated that potassium carbonate was dispersed on the surface of the straw or into the cellulosic internal structure after immersion. It was reported that around 700 °C, the reaction (3) would occur.24 The metallic K could further develop porosity by intercalation through carbon sheets to enlarge the pores. Due to the removal of tarry material within the pores, microporous and mesoporous could also be developed at the temperature blow 600 °C.23
K2CO3 + 2C → 2K + 3CO | (3) |
Under high temperature conditions, potassium carbonate catalyzed the gasification of cellulose,23 and the small amount of potassium carbonate that attached to the biomass surface reacted with the surrounding cellulose molecules, leaving the non-penetrating pits. This structure was clearly observed in the electron microscopy of KBC450, KBC600 and KBC750, but not on the surface of BC600. If the amount of potassium carbonate that attached to the surface was sufficient, potassium carbonate would react with cellulose continuously and form penetrating pores. The potassium carbonate inside the cellulose would leave pores in the interior and cross link with each other. The higher the temperature, the more complete the gasification reaction, the higher the pores density. The porous property of KBC was more favorable to the diffusion of pollutants into the interior, which has positive significance to improve the adsorption characteristics.
The specific surface area and pore size parameters of KBC and BC600 are shown in Table 2. The activation effect of potassium carbonate was affected by the pyrolysis temperature. With the increasing pyrolysis temperature, the specific surface area and total pore volume of KBC were increased. The BET surface area of KBC750 was the highest, reached 814.89 m2 g−1. When the pyrolysis temperature was 450 °C, the specific surface area and pore volume of micropores were smaller than mesoporous and macropore. When the pyrolysis temperature was rising to 600 °C and 750 °C, the specific surface area and pore volume of micropores were larger than mesoporous and macropore. It showed that potassium carbonate mainly increased the mesoporous and macroporous at low pyrolysis temperature, and the micropores would increase when the activation temperature was high. The average pore size decreased with the increase of activation temperature, which indicated that the possibility of micropores increased with the rising activation temperature.
Sample | KBC450 | KBC600 | KBC750 | BC600 |
---|---|---|---|---|
a SBET stands for BET specific surface area; VT for total pore volume; Sex for t-plot external specific surface area; Smic for t-plot micropore specific surface area; Sm for mesoporous and macroporous surface area; Vmic for t-plot micropore volume; Vm for mesoporous and macroporous pore volume. | ||||
SBET (m2 g−1) | 57.80 | 541.91 | 814.89 | 86.75 |
VT (mL g−1) | 0.081 | 0.339 | 0.478 | 0.079 |
Sex (m2 g−1) | 46.57 | 114.77 | 125.85 | 60.38 |
Smic (m2 g−1) | 11.23 | 427.14 | 689.04 | 26.37 |
Sm (m2 g−1) | 33.69 | 71.46 | 72.61 | 19.99 |
Vmic (mL g−1) | 0.004 | 0.198 | 0.32 | 0.012 |
Vm (mL g−1) | 0.072 | 0.124 | 0.143 | 0.03 |
BET average pore width (nm) | 4.91 | 2.38 | 2.27 | 3.79 |
Potassium carbonate had a significant effect on the specific surface area and pore structure. Compared with the unactivated biochar, the specific surface area of KBC600 was 5 times that of BC600, and the total pore volume, micropores area and outward surface area of KBC600 were significantly larger than BC600. The BET average pore size of BC600 was greater than that of KBC600 and KBC750, indicating that the addition of potassium carbonate may increase the distribution of micropores. Compared with other activators, biochar was significantly activated by potassium carbonate. The specific surface area of biochar that activated by KOH at 500 °C was only 59 m2 g−1,27 meanwhile HCl activated kenaf fibre char was 346.5 m2 g−1,28 and H3PO4 activated biochar derived by corn stalk under 550 °C had mesoporous structure with SBET of 600 m2 g−1.29 The specific surface area of KBC600 and KBC750 prepared by this method was significantly larger. Over all, using potassium carbonate as the activator has a significant effect on increasing the pore complexity of biochar, forming and optimizing the composite pore structure. This effect was more prominent at high temperature.
Fig. 3 shows the mesoporous pore size distribution of KBC and BC600. The result suggested that the pores of KBC were distributed centrally over 2–4 nm and 6–125 nm. Compared with KBC, the mesoporous distribution of BC in the range of 3–9 nm was more than that of KBC, but the mesoporous distribution with larger pore size (8–50 nm) wasn't dominant. With the increase of pyrolysis temperature, the number of microporous, pore density and specific surface area were increased, which showed that potassium carbonate played a role in increasing both the internal micropores and mesopores distribution. The macroporous spread on the exterior densely, and the micro–mesopore composite structure distributed on the inner surface would facilitate the diffusion of contaminant molecules into the biochar.
Sample | Langmuir | Freundlich | ||||
---|---|---|---|---|---|---|
b/L mg−1 | qm/mg g−1 | R2 | kf | 1/n | R2 | |
KBC450 | 0.370 | 63.25 | 0.9922 | 22.23 | 0.372 | 0.9898 |
KBC600 | 1.92 | 70.05 | 0.9962 | 47.10 | 0.184 | 0.9909 |
KBC750 | 15.56 | 130.70 | 0.9761 | 123.79 | 0.153 | 0.9945 |
BC600 | 0.214 | 43.06 | 0.9943 | 14.49 | 0.302 | 0.9973 |
The correlation analysis was used to analyze the influence of the chemical and structural properties of the biochar on the adsorption performance. The results are shown in Table 4. kf is the adsorption constant of Freundlich model, and its value is related to the adsorption capacity and adsorption strength. n could characterize the interaction strength between adsorbate and adsorbent surface, and the larger the value of n, the stronger the interaction.31 There was a negative correlation between H/C and qm, and the negative correlation between H/C and n, kf reached a significant level, indicating that the increase of aromaticity would enhance the affinity of naphthalene with biochars surface and promote the adsorption of naphthalene to form larger adsorption capacity. There was also a similar relationship between O/C, (O + N)/C and qm, n, kf, which mean that the adsorption of naphthalene by KBC was significantly related to the hydrophilicity and polarity of biochar, and the non-polar hydrophobic surface was more conducive to the adsorption of naphthalene. The polarity and hydrophilicity of biochar occupy the dominant position in the adsorption of naphthalene, and the increase in oxygen-containing functional groups, such as carbonyl, carboxyl, and ether groups, reduces the sites available for naphthalene adsorption on the surface.32
H/C | O/C | (O + N)/C | SBET | VT | Vmic | Vmes | Average pore width | n | kf | |
---|---|---|---|---|---|---|---|---|---|---|
a *indicates significant correlation at p < 0.05 level. **indicates significant correlation at p < 0.01 level. | ||||||||||
O/C | 0.843 | |||||||||
(O + N)/C | 0.791 | 0.991** | ||||||||
SBET | −0.963* | −0.839 | −0.821 | |||||||
VT | −0.953* | −0.846 | −0.832 | 0.999** | ||||||
Vmic | −0.966* | −0.852 | −0.832 | 1.000** | 0.999** | |||||
Vmes | −0.804 | −0.860 | −0.892 | 0.921 | 0.936 | 0.921 | ||||
Average pore width | 0.865 | 0.539 | 0.509 | −0.909 | −0.900 | −0.899 | −0.749 | |||
n | −0.957* | −0.781 | −0.759 | 0.995** | 0.992** | 0.992** | 0.893 | −0.946 | ||
kf | −0.964* | −0.954* | −0.915 | 0.927 | 0.924 | 0.936 | 0.838 | −0.722 | 0.895 | |
qm | −0.907 | −0.990* | −0.963* | 0.880 | 0.881 | 0.892 | 0.844 | −0.616 | 0.832 | 0.986* |
SBET, VT, Vmes, Vmic and qm, n, kf showed a positive correlation. It was noteworthy that the specific surface area of KBC600 was 9.38 times that of KBC450, but the saturation adsorption capacity fitted by Langmuir equation was similar. Similarly, the specific surface area of BC600 was 1.5 times that of KBC450, but the maximum adsorption capacity was lower than that of KBC450. When the pyrolysis temperature was raised to 750 °C, the specific surface area of KBC750 increased by 1.5 times compared with that of KBC600, but the adsorption capacity increased nearly twice. The above observations showed that the specific surface area was not the only determinant of naphthalene adsorption by KBC, surface chemical properties also play an important role. The improvement of pore structure, such as the increase of mesopores and micropores, would promote the diffusion of naphthalene and its interaction with the surface of biochars, forming a larger adsorption capacity. Micropore volume had a very significant positive correlation with total pore volume and specific surface area, indicating that micropores played a key role in promoting the formation of large surface area and large pore volume. The average pore size was negatively correlated with qm, n and kf. The increase of the average pore size means the formation of pore with larger size, which would reduce the number of micropores and mesopores, leading to the decrease of specific surface area. It was also illustrated by the negative correlation between average pore size and SBET. The biochar activated by potassium carbonate had a marked increase in surface aromaticity, hydrophobicity and non-polarity, as well as richer pore structure and larger specific surface area, so the adsorption capacity for naphthalene was greater.
Except for alkyl groups, the major oxygen-containing functional groups of KBC450 and KBC600 did not disappear as the pyrolysis temperature increasing (Fig. 5). This was one of the reasons why there was no difference between O/C and (O + N)/C for KBC450 and KBC600. As the pyrolysis temperature increases, the oxygen-containing functional groups on the KBC surface gradually decreased. When the temperature was raised to 750 °C, the absorption peak of hydroxyl group33 and carboxyl group CO34 disappeared, and the absorption peak of carboxyl group and ether bond16 was strongly impaired. The disappearance of the aromatic C–H vibration35 indicated that the carbon atoms were arranged more closely. High pyrolysis temperature coursed the graphitization of KBC. These changes were conducive to the formation of non-polar hydrophobic surface. Before and after the adsorption of naphthalene, there was no obvious change in the infrared spectrum of biochar surface except for the displacement of absorption peak wavenumber of oxygen functional group (Fig. 5). It suggested that naphthalene adsorbed on the surface of KBC may not form a new chemical bond, but it was fixed on the KBC surface by conjugation or van der Waals force.36,37 The aromatic structure of naphthalene can serve as an electron donor and undergo π–π electron-donor–acceptor (π–π EDA) interaction with the electron-deficient aromatic structure on the surface of KBC.38 For example, the absorption peak at 1158 cm−1 was due to the C–O–C stretching vibration associated with the aromatic ring/olefin.39 After adsorption of naphthalene by KBC, the absorption peak shifted to high frequency, indicating the interaction between naphthalene and the oxygen-containing functional groups of biochar and the existence of π–π EDA.40
This journal is © The Royal Society of Chemistry 2018 |