Xiaobo Chen*a,
Jingguo Dinga,
Yan Lia,
Yinxia Wua,
Guoce Zhuanga,
Cuicui Zhanga,
Zhihai Zhanga,
Chengyun Zhua and
Peizhi Yang*b
aSchool of New Energy and Electronic Engineering, Yancheng Teachers University, Yancheng, 224051, PR China. E-mail: chenxbok@126.com
bKey Laboratory of Education Ministry for Advance Technique and Preparation of Renewable Energy Materials, Institute of Solar Energy, Yunnan Normal University, Kunming, 650500, PR China. E-mail: pzhyang@hotmail.com
First published on 19th July 2018
NiCoSe2 microspheres have been successfully synthesized by a facile one-step hydrothermal method at different hydrothermal temperatures. The prepared samples are divided according to their reaction temperatures (90, 120, 150 and 180 °C) and named NiCoSe2-90, NiCoSe2-120, NiCoSe2-150 and NiCoSe2-180, respectively. The diameters of the NiCoSe2 microspheres strongly depend on the different hydrothermal temperatures. When the temperature is increased to 150 °C, the size of the resultant NiCoSe2 microspheres changes from 200 to 800 nm, and the interior of NiCoSe2-150 possesses a flocculent structure. However, NiCoSe2-180 displays a cauliflower-like aggregated structure. The prepared NiCoSe2 alloys are used as high-performance Pt-free counter electrodes (CEs) for dye-sensitized solar cells (DSSCs). Cyclic voltammogram measurement indicates that NiCoSe2-150 CE has larger current density than Pt CE. Electrochemical impedance spectroscopy shows that NiCoSe2-150 CE has a low charge-transfer resistance of 1.8 Ω cm2. Due to their unique morphologies and well-defined interior and exterior structures, DSSCs based on NiCoSe2-120 and NiCoSe2-150 CEs achieve high power conversion efficiencies of 8.48% and 8.76%, respectively, which are higher than that of the solar cell based on Pt CE (8.31%).
Several low-cost materials with excellent performances, such as alloys,8,9 transition metal compounds,4,10,11 carbonaceous materials,12,13 composites,14,15 and conductive polymers,16,17 have been successfully utilized as Pt-free CEs in DSSCs. Among these Pt-free CE materials, metal selenides are competitive candidates because of their outstanding electrocatalytic activity for triiodide reduction.4,18–20 A hollow NiSe–Ni3Se2 hybrid nanostructure composite was also directly synthesized on reduced graphene oxide in situ; the NiSe series exhibited a high PCE value of 7.87%.21 Profiting from the coexistence of Ni and Co in Ni–Co selenides, ternary selenides offer richer redox reactions than NiSe and CoSe. For example, (Ni1−xCox)Se2 nanoparticles were synthesized via a one-step hydrothermal reduction route, and the obtained sample could exhibit better electrocatalytic properties compared to NiSe2, CoSe2 and Pt.22 Moreover, it is generally acknowledged that stoichiometric ratio and morphology are the two main factors that affect the catalytic activity of CE materials.
Herein, NiCoSe2 microspheres were prepared by a one-step facile hydrothermal method at different hydrothermal temperatures, and they were used as CE materials for DSSCs. The size of the microspheres increased with the increase in the reaction temperature, and the microspheres exhibited agglomeration. Meanwhile, the NiCoSe2-150 sample exhibited the most porous features. The overall energy conversion efficiency of the DSSC with NiCoSe2-150 CE reached 8.76%, and DSSCs with NiCoSe2-120 and NiCoSe2-180 CEs achieved power conversion efficiencies (PCE) of 8.48% and 8.31%, respectively. PCEs of the cells based on the above-mentioned three NiCoSe2 CEs were superior to that of Pt CE-based DSSC (8.22%).
Electrochemical analyses, including cyclic voltammetry (CV) measurements, Tafel polarization curves and electrochemical impedance spectroscopy (EIS), were conducted on an electrochemical workstation (CHI660E, Shanghai Chenhua Device Company, China). Cyclic voltammetry measurements were performed in a three-electrode system in an acetonitrile solution of 1 mM I2, 10 mM LiI and 100 mM LiClO4, and the potential range was set from −0.6 V to 1.2 V at a scan rate of 50 mV s−1. The FTO glass coated with the catalyst was used as the working electrode; a Pt foil and an Ag/AgCl electrode were used as the counter electrode and the reference electrode, respectively. Tafel polarization curves and electrochemical impedance spectroscopy results were obtained using a symmetrical cell consisting of two same NiCoSe2 alloy electrodes (CE/electrolyte/CE). EIS was performed in the frequency range from 100 kHz to 100 mHz with 5 mV amplitude. Tafel polarization curves were scanned from −1.0 to 1.0 V with a scan rate of 10 mV s−1. Moreover, the resultant impedance spectra were analyzed by the Z-view software. The incident photon conversion efficiencies (IPCE) were obtained using a Keithley 2000 SourceMeter under the irradiation of a 150 W xenon lamp (Oriel) fitted with a monochromator (Cornerstone 74004) as the monochromatic light source. The photocurrent–voltage (J–V) characteristics of DSSCs based on the as-prepared CEs and commercial Pt/FTO CE were conducted by a standard solar simulator (Xe Lamp Oriel Sol3A™ Class AAA Solar Simulators 94023A, USA) under irradiation of simulated solar light at ambient atmosphere. The J–V curves were also recorded by the CHI660E electrochemical workstation.
SEM images were obtained for the investigation of the structural morphologies of the synthesized samples. As shown in Fig. 2a, NiCoSe2-90 was composed of a large number of dense spherical particles with a diameter of about 200 nm. When the hydrothermal temperature was increased to 150 °C, the size of NiCoSe2 spheres became larger; this was consistent with the XRD analysis. The SEM image of NiCoSe2-150 (Fig. 2c) revealed that NiCoSe2 spheres with a diameter of about 800 nm were obtained as some of the spheres were partially broken, which can be clearly observed from the flocculent structure of the as-synthesized NiCoSe2 spheres. Moreover, the unique flocculent structure of the NiCoSe2-150 sample could provide effective transport pathways for electrons and ions, which enhanced the electrochemical kinetics. However, NiCoSe2-180 (Fig. 2d) displayed a cauliflower-like aggregated structure since the spheres were connected to each other, and it was difficult to separate out a single sphere, which might have been affected by the relatively high temperature of the hydrothermal process. The atomic ratios of the prepared Ni–Co–Se alloys were determined by EDS using NiCoSe2-150 as a representative sample. The elemental concentrations of Ni, Co and Se in the film were ascertained as 25.1, 27.3 and 47.6, respectively. This ratio was close to the composition of NiCoSe2 (1:1:2). Furthermore, as can be seen in Fig. 2e–h, Ni, Co and Se elements displayed a uniform distribution in the mapping diagram, which further confirmed that the Ni–Co–Se alloys have been successfully synthesized. The TEM image (Fig. 2j) further confirmed the sphere size and the overall morphology of NiCoSe2-150. The typical HRTEM image (the inset of Fig. 2j) revealed clear lattice fringes separated by 0.371 nm and 0.266 nm, corresponding to the (110) plane of orthorhombic CoSe2 and the (202) plane of monoclinic Ni3Se4, which agreed well with the XRD results.
To investigate the chemical bonding states and the elemental components of the NiCoSe2 alloy, the sample was examined by X-ray photoelectron spectroscopy (XPS). The NiCoSe2-150 sample was selected as a representative sample. As shown in Fig. 3a, the survey spectrum confirmed the presence of C, O, Ni, Co and Se in the product. The C 1s peak and the O 1s peak appeared because the surface was exposed in ambient conditions, and it adsorbed other elements inevitably, which indicated that the near-surface of the NiCoSe2-150 sample mainly comprised Se, Ni, and Co.25 Fig. 3b–d show the high-solution XPS spectra of Ni 2p, Co 2p and Se 3d, respectively. The high-solution spectra of Ni 2p and Co 2p could be divided into spin–orbit doublets and shakeup satellites (identified as “Sat.”) by the Gaussian fitting method. The Ni 2p spectrum of NiCoSe2-150 is shown in Fig. 3b; the fitting peak at 853.3 was assigned to Ni2+, and the peak at 872.5 eV was ascribed to Ni3+.26,27 For the Co spectrum, the first doublet (at 777.9 and 792.6 eV) and the second doublet (at 779.7 and 795.1 eV) were the characteristics of Co3+ and Co2+.25,28 Our results showed that the Co and Ni atoms were in divalent states. Moreover, as shown in Fig. 3d, Se 3d peaks could be deconvoluted into two peaks; the two peaks at 59.2 eV and 55.3 eV could be assigned to Se 3d3/2 and 3d5/2, respectively, which represented typical metal–selenium bonds.29 According to the XPS analysis, it was clear that the surface of the Ni–Co–Se alloy mainly consisted of Ni2+, Co2+ and Se2−.
3I2 + 2e− ↔ 3I− | (1) |
I3− + 2e− ↔ 3I− | (2) |
The I3− reduction reaction mainly occurs on the side of CE; thus, the I−/I3− redox couple was explored in this study. Generally, the peak-to-peak potential separation (Epp) between Red-1 and Ox-1 and the peak current density of the reduction peak Red-1 (|JRed-1|) are two crucial parameters in a CV curve. Moreover, the value of |JRed-1| is always utilized to assess the reaction rate of the CE catalyst for the reduction reaction of I3− to I−. A higher peak current density |JRed-1| results in enhanced electrocatalytic activity of the CE material. As shown in Table 1, NiCoSe2-150 CE possessed the highest |JRed-1| value of 4.31 mA cm−2, suggesting that this sample has higher I−/I3− redox couple electrocatalytic ability compared to Pt (3.59 mA cm−2). Moreover, the |JRed-1| value of NiCoSe2-120 (3.81 mA cm−2) was slightly larger than that of Pt CE. On the other hand, Epp is a parameter to evaluate the reversibility of the redox reaction, and a lower Epp value means better electrocatalytic ability. The Epp values of CEs increased in the order NiCoSe2-150 (461 mV) < NiCoSe2-120 (465 mV) < NiCoSe2-180 (487 mV) < Pt (535 mV) < NiCoSe2-90 (633 mV). Apparently, NiCoSe2-120 and NiCoSe2-150 CEs showed significantly higher electrocatalytic activities than Pt. Additionally, the highest |JRed-1| and lowest Epp values indicated that NiCoSe2-150 CE has superior electrocatalytic activity for I3− reduction, due to which it can be a better alternative material to Pt CE in DSSCs.
CEs | Epp (mV) | |JRed-1| (mA cm−2) | Rs (Ω cm2) | Rct (Ω cm2) | J0 (mA cm−2) | Jlim (mA cm−2) |
---|---|---|---|---|---|---|
NiCoSe2-90 | 633 | 3.28 | 9.4 | 12.5 | 1.28 | 33.73 |
NiCoSe2-120 | 465 | 3.81 | 9.6 | 3.1 | 6.53 | 84.72 |
NiCoSe2-150 | 461 | 4.31 | 9.6 | 1.8 | 10.67 | 118.85 |
NiCoSe2-180 | 487 | 3.43 | 9.5 | 2.5 | 7.41 | 99.54 |
Pt | 535 | 3.59 | 9.5 | 6.2 | 5.46 | 79.07 |
In addition, Fig. 4b shows CVs of the I−/I3− system on the NiCoSe2-150 electrode with different scan rates (i.e., 50, 75, 100 and 125 mV s−1). With the increasing scan rate, CVs exhibit a regularly outward extension of all peaks. Fig. 4c illustrates the linear relationship between the peak current density and the square root of the scan rate, indicating that the diffusion of I− controls the redox reaction on CE and there is no specific interaction between the prepared CE and the I−/I3− redox pair.31 To investigate the stability of CE in the liquid electrolyte, CV measurements have been performed on the CE based on NiCoSe2-150 at a scan rate of 50 mV s−1 for 100 cycles (see Fig. 4d). No apparent decrease in the current density is observed during cycling, indicating that this CE exhibits good electrochemical stability as the CE material for DSSCs.
EIS analysis was conducted using typical symmetrical dummy cells for further characterization of the charge transfer process at the electrolyte/CE interface. Nyquist plots of all cells with Ni–Co–Se alloy CEs (Fig. 5a) showed two semicircles at the low-frequency and the high-frequency regions. The intercept of the high-frequency semicircle with the horizontal axis signifies the series resistance (Rs), which can be affected by the adhesion of the electrocatalyst film to the FTO glass. The high-frequency semicircle corresponds to the charge transfer resistance (Rct) at the CE/electrolyte interface for the I3− reduction, which is a pivotal parameter reflecting the catalytic activity of the prepared CEs. A smaller value of Rct stands for a smaller value of the overpotential needed for the electron transfer from CE to electrolyte.32,33 The low-frequency semicircle (right-hand side) represents the Warburg diffusion resistance (ZW) within the bulk electrolyte and the electrocatalyst film. The above-mentioned parameters were extracted by fitting the EIS spectrum with an equivalent circuit (the inset of Fig. 5a), and the results are shown in Table 1. As shown in Table 1, the Rs values of NiCoSe2-90, NiCoSe2-120, NiCoSe2-150, NiCoSe2-180 and Pt were 9.4, 9.6, 9.6, 9.5 and 9.5 Ω cm2, respectively. A larger Rs value indicates weaker adhesion of the electrocatalytic material to the FTO substrate. All Rs values were very close to each other. In addition, Rct increased in the order NiCoSe2-150 (1.8 Ω cm2) < NiCoSe2-180 (2.5 Ω cm2) < NiCoSe2-120 (3.1 Ω cm2) < Pt (6.2 Ω cm2) < NiCoSe2-90 (12.5 Ω cm2), which indicated that the Rct values of NiCoSe2-120, NiCoSe2-150 and NiCoSe2-180 were all smaller than that of Pt. It is thus apparent that the above-mentioned three devices have higher catalytic activities and charge-transfer abilities than the Pt-based DSSC.
Tafel polarization analysis was carried out to estimate the electrocatalytic activity of the charge-transfer performance of the I−/I3− redox pair at the CE/electrolyte interface. Typically, a Tafel curve can be divided into three zones by the value of the overpotential. The region at the lower overpotential of |U| < 0.120 V represents the polarization zone, the region at the middle potential with a sharp slope represents the Tafel zone, and the region at higher overpotential with the horizontal portion represents the diffusion zone. The exchange current density (J0) is estimated from the slope of the cathodic or the anodic branch, and the limiting diffusion current density (Jlim) is the intersection of the anodic branch with the Y-axis. J0 and Jlim can be obtained from the corresponding Tafel zone and the diffusion zone.34–37 As shown in Fig. 5b, NiCoSe2-150 CE achieved the highest J0 value (10.67 mA cm−2) in the Tafel zone, and it exhibited the strongest catalytic activity. The J0 values for these electrodes followed the order NiCoSe2-150 > NiCoSe2-180 > NiCoSe2-120 > Pt > NiCoSe2-90, suggesting that the catalytic activities of CEs could be presented in the same order. In the diffusion region, NiCoSe2-120, NiCoSe2-150 and NiCoSe2-180 CEs exhibited higher Jlim values compared to Pt, which indicated that these prepared electrodes can achieve higher catalytic activities. NiCoSe2-90 CE showed the lowest Jlim value, which suggested the lowest electrocatalytic ability towards I3− reduction. The trend of Jlim was consistent with that of J0 for these CEs. Additionally, the J0 values could be calculated by using eqn (3), and the parameters obtained from the Tafel plots are given in Table 1. Larger J0 values result in smaller Rct values of CEs, which was in agreement with the EIS data. Clearly, the above-mentioned CV, EIS, and Tafel polarization measurement results indicated that the NiCoSe2-150 electrode had the highest catalytic activity as a CE compared to the other NiCoSe2 CEs and Pt CE. In contrast, NiCoSe2-120, NiCoSe2-150, NiCoSe2-180 showed higher catalytic activities than Pt and exhibited potentials to achieve reasonably high PCE values.
J0 = RT/nFRct | (3) |
Fig. 6 (a) J–V curves (b) IPCE curves of DSSCs with NiCoSe2-90, NiCoSe2-120, NiCoSe2-150, NiCoSe2-180 and Pt-based CEs. |
CEs | Voc (V) | Jsc (mA cm−2) | FF | PCE (%) |
---|---|---|---|---|
NiCoSe2-90 | 0.786 ± 0.014 | 15.65 ± 0.011 | 0.615 ± 0.010 | 7.56 ± 0.25 |
NiCoSe2-120 | 0.760 ± 0.012 | 17.44 ± 0.011 | 0.640 ± 0.011 | 8.48 ± 0.24 |
NiCoSe2-150 | 0.770 ± 0.008 | 17.82 ± 0.007 | 0.638 ± 0.009 | 8.76 ± 0.22 |
NiCoSe2-180 | 0.774 ± 0.012 | 17.08 ± 0.011 | 0.628 ± 0.010 | 8.31 ± 0.26 |
Pt | 0.765 ± 0.010 | 16.84 ± 0.008 | 0.637 ± 0.009 | 8.22 ± 0.21 |
To analyse the differences between the Jsc values of these devices, the IPCE responses as a function of the incident wavelength are plotted in Fig. 6b. The IPCE plot of the DSSC based on NiCoSe2-150 covers a broad wavelength range from 400 nm to 800 nm with an IPCE maximum value of 89.9% at 530 nm, and this value matches well with the absorption result of the commercial N719 dye. Moreover, the order of the IPCE values for these devices is NiCoSe2-150 > NiCoSe2-120 > NiCoSe2-180 > Pt > NiCoSe2-90, which agrees well with the Jsc order. With the increase in the hydrothermal temperature, PCEs of NiCoSe2-based DSSCs increase first and then decrease with a maximum value of 8.76%. The high IPCE value and the broader absorption of NiCoSe2-150 explain the high Jsc value from the J–V measurement. The slightly higher efficiency observed for NiCoSe2-150 is mainly due to relatively larger Jsc value, which can be due to the efficient reduction of I3− and the reduced charge transfer resistance at the CE/electrolyte interface. NiCoSe2-150 CE exhibits superior morphology, which is beneficial to enhance its catalytic activity.
This journal is © The Royal Society of Chemistry 2018 |