Open Access Article
This Open Access Article is licensed under a
Creative Commons Attribution 3.0 Unported Licence

Low temperature synthesis of BiFeO3 nanoparticles with enhanced magnetization and promising photocatalytic performance in dye degradation and hydrogen evolution

M. A. Basith*, Nilufar Yesmin and Rana Hossain
Department of Physics, Bangladesh University of Engineering and Technology, Dhaka-1000, Bangladesh. E-mail: mabasith@phy.buet.ac.bd

Received 29th May 2018 , Accepted 14th August 2018

First published on 21st August 2018


Abstract

In this investigation, we have synthesized BiFeO3 nanoparticles by varying hydrothermal reaction temperatures from 200 °C to 120 °C to assess their visible-light driven photocatalytic activity along with their applicability for hydrogen production via water splitting. The rhombohedral perovskite structure of BiFeO3 is formed for hydrothermal reaction temperature up to 160 °C. However, for a further decrement of hydrothermal reaction temperature a mixed sillenite phase is observed. The XRD Rietveld analysis, XPS analysis and FESEM imaging ensure the formation of single-phase and well crystalline nanoparticles at 160 °C reaction temperature with 20 nm of average size. The nanoparticles fabricated at this particular reaction temperature also exhibit improved magnetization, reduced leakage current density and excellent ferroelectric behavior. These nanoparticles demonstrate considerably high absorbance in the visible range with a low band gap (2.1 eV). The experimentally observed band gap is in excellent agreement with the calculated band gap using first-principles calculations. The favorable photocatalytic performance of these nanoparticles has been able to generate more than two times of solar hydrogen compared to that produced by bulk BiFeO3 as well as commercially available Degussa P25 titania. Notably, the experimentally observed band gap is almost equal for both bulk material and nanoparticles prepared at different reaction temperatures. Therefore, in solar energy applications, the superiority of BiFeO3 nanoparticles prepared at 160 °C reaction temperature may be attributed not only to their band gap but also to other factors, such as reduced particle size, excellent morphology, good crystallinity, large surface to volume ratio, ferroelectricity and so on.


1 Introduction

Nanotechnology has had a tremendous impact in contribution to the solution of the local as well as global energy crisis by converting sunlight directly into electric/chemical power. A promising area for the application of nanotechnology is the hydrogen economy. As a non-polluting source of energy, hydrogen (H2) can be a good alternative fuel of the future1–3 without polluting the environment. H2 production can be performed from different domestic feedstocks including hydrocarbon fossil fuels and water. Notably, H2 produced by splitting of water4–6 under solar light illumination is of great promise as a fuel that is essentially carbon free and inexhaustible in nature with potential for generating low cost power in power plants as well as in next generation.

Photocatalytic disintegration of water7 into H2 and O2 while irradiated by light in the visible region has been considered as one of the promising routes for H2 production as an endless source of clean fuel for many applications. In 1972, Fujishima and Honda successfully used titania (TiO2) photoelectrode for the decomposition of water3 under illumination with sunlight and without any applied electric power. Since then many propositions along with numerous researches have been conducted on hydrogen production via water splitting.8 In the past decade, extensive studies were performed on a broad range of materials, including modified TiO2,9 SrTiO3 (ref. 10) and metal oxide–metal hybrids like ZnO/(La,Sr)CoO3 (ref. 11) and CdS/TiO2/Pt12 to improve their photocatalytic water splitting ability under UV-visible light irradiation. Recently, significant amount of research is being done with a view to improving the photocatalytic activity of the multiferroic materials such as bismuth iron oxide (BiFeO3) to investigate its potentiality for solar hydrogen generation.1,13 BiFeO3 (BFO) intrigues with its multiferroic properties being potentially applicable in energy-related problems especially for photocatalytic hydrogen production imputed to its relatively small band-gap (2.6 eV).14–17 It is reported that BiFeO3 generates hydrogen at a greater amount than commercially available titania under exact parametric conditions.13 Utilization of a somewhat broader sunlight spectrum along with a large polarization value of BFO efficiently generated electron–hole pairs.18 Notably, BFO could potentially supplant the widely investigated photocatalyst TiO2 that has an inherent limitation of wide band gap (3.2 eV), qualifying its utilization to only 4% of the solar spectrum.19 Despite the great potential it possesses, the somewhat inferior photocatalytic performance of bulk BiFeO3 restrains its commercialization.20,21

Multiferroic BiFeO3 was discovered in 1960, however, it remains difficult to synthesize single phase BFO nanoparticles with excellent morphology owing to the fact that the temperature range for stability is in fact quite narrow for this material. If the synthesis condition, particularly the processing temperature is not subject to accurate control, other impurity phases such as Bi2Fe4O9 appears in BFO nanoparticles. Therefore, a number of synthesis techniques for BFO nanoparticles have been developed at different temperatures. These include soft chemical routes (e.g. sol–gel method),22 ultrasonication technique,23 microemulsion technique24 and microwave-hydrothermal process.25 Most of these synthesis techniques, inherently cost inefficient, comprise of higher than 400 °C calcination temperatures for achieving phase purity for BFO which introduces irregular morphology and broad particle size distribution. While sol–gel has gained popularity among different wet chemical techniques, it has a stringent requirement of an annealing temperature of 600 °C as the concluding step as well as a post treatment similar to solid-state synthesis techniques for elimination of impurity phases. Combustion synthesis can yield nanosized BFO powder at the expense of phase purity26 being inferior to the ones synthesized by the soft chemical route.22 Hence, synthesis of phase pure BFO nanoparticles at a moderate preparation condition has become quite challenging. Since many years, hydrothermal synthesis of phase pure BFO powders gained intensive research interest due to its potential in synthesizing crystalline ceramics at a temperature of 200 °C or even lower without any further step of calcination. This is a cost effective and simple method, and the primacy of this technique is that it requires significantly lower temperature than both solid-state and sol–gel syntheses. During the preparation of BFO, such a low processing temperature qualifies the reactants from getting volatilized as well as minimizing the calcination introduced impurities.

Therefore, it is obvious that enormous effort was paid to conduct extensive research to synthesize pure BFO nanoparticles using hydrothermal technique. However, there is still lack of a thorough investigation on synthesis, characterization and application of pure BFO nanoparticles with desired phase and crystallinity prepared at very low temperature using a facile, low cost synthesis route like hydrothermal. It is indeed very essential to shed light to know different crystallographic phases formed at different reaction temperatures and finally figure out the appropriate reaction temperature to obtain phase pure BFO nanoparticles ensuring their quality as required for practical applications. In this investigation, we delineate the synthesis of BFO nanoparticles adapting a facile hydrothermal process for different reaction temperatures and a fixed KOH concentration of 10 M.27 With a view to knowing the crystallographic phases, we scrutinized Rietveld refinement on powder XRD data of the samples synthesized over a wide range of temperatures varying from 200 °C to 120 °C. Notably, in most of the previous hydrothermal investigations either crystallographic phases of BFO nanoparticles were not identified by Rietveld or related analysis and/or it was done at a particular temperature27,28 not like here over a wide range of temperatures. We observed that well-dispersed, single-phase perovskite BFO nanoparticles with average particle size 20 nm can be produced by hydrothermal process at temperature as low as 160 °C (from here this material is referred as BFO 160 unless otherwise specified). A further reduction of temperature to 140 °C did not allow fabrication of single phase perovskite structure rather produced sillenite type mixed phases nanoparticles. Interestingly, the single-phase BFO 160 nanoparticles demonstrate excellent multiferroic, optical and photocatalytic properties. The hydrogen evolution experiment exhibited that BFO 160 nanoparticles generated more than two times hydrogen than that of BFO bulk material and commercially available TiO2 under the same experimental conditions.

2 Experimental details

2.1 Sample preparation

In the present investigation, the chemical reagents are analytical grade bismuth nitrate (Bi(NO3)3·5H2O), ferric nitrate (Fe(NO3)3·9H2O), and potassium hydroxide (KOH). In a typical procedure, 1 mmol bismuth nitrate pentahydrate [Bi(NO3)3·5H2O] and 1 mmol ferric nitrate nonahydrate [Fe(NO3)3·9H2O] in stoichiometric proportions were dissolved in 50 ml of 10 M KOH solution and stirred it for 4 h.27–29 The mixture was transferred to a Teflon-lined autoclave (stainless steel, capacity 100 ml) and was heated at different reaction temperatures between 200 °C to 120 °C for 6 hours followed by natural cooling to bring it to room temperature. Centrifugation was applied to collect the final products and consequent rinsing was performed with distilled water and ethanol. Prior to further characterization, they were dried at 90 °C for 6 hours. Bulk BiFeO3 sample had also been prepared from high purity oxides using solid state reaction method with an objective of comparing its properties to the synthesized nanoparticles.30

2.2 Materials characterization

The crystal structures and phase composition of the synthesized samples were determined from XRD data using a diffractometer (PANalytical Empyrean) with a Cu X-ray source (Wavelength, λ: Kα1 = 1.540598 Å and Kα2 = 1.544426 Å. The particle size along with morphology was observed with help of field emission scanning electron microscopy (FESEM) (XL30SFEG; Philips, Netherlands and S4300; HITACHI, Japan). X-ray photoelectron spectroscopy (XPS) was used to investigate the chemical states of synthesized nanoparticles. A vibrating sample magnetometer (VSM) was used for measuring the magnetic properties of the BFO powders at room temperature. The leakage current density along with polarization vs. electric field hysteresis loops were measured using a ferroelectric loop tracer in conjunction with external amplifier (10 kV). Pellets were prepared by pressing the powders with a hydraulic press followed by annealing at 750 °C with high heating rate (20 °C min−1) with a view to measuring the electrical properties.31 An ultraviolet-visible (UV-vis) spectrophotometer (UV-2600, Shimadzu) was used to obtain diffuse reflectance spectra (DRS) of the samples for wavelength ranging from 200 to 800 nm. BaSO4 powder, a nonabsorbing standard material, was used as the reference for total reflectance with the focused beam spot size being approximately of 2 mm2.

2.3 Theoretical calculation of optical properties

With a view to understanding the optical properties of BFO bulk and BFO 160 nanoparticles, the optical absorption was calculated based on crystallographic structural parameters obtained from Rietveld refinement32 of this investigation. The calculations were performed using first-principles density functional theory (DFT) within the plane wave pseudopotential (PWPP) framework as implemented in the Cambridge Serial Total Energy Package (CASTEP).33 The generalized gradient approximation (GGA) with the Perdew–Burke–Ernzerhof (PBE) exchange–correlation functional within ultrasoft pseudopotentials (USP) was implemented to describe the electron–ion interaction of valance electrons of Bi(6S26p3), Fe(3d64s2) and O(1s22p4).34 Plane wave cutoff and k-point sampling, tested with a cutoff of 400 eV and a k-point sampling of 6 × 6 × 6, was found sufficient for the rhombohedral unit cell of the samples. Spin polarized mode during self-consistent field (SCF) calculations was endorsed and a SCF tolerance of 10−7 eV per atoms was used. To assure a precise agreement with experimental results, the on-site Coulomb interaction was included in the DFT+U approach with U = 3 eV to 7 eV with interval 0.5 eV for Fe 3d orbital.35 The optical absorption coefficient was obtained by the equation image file: c8ra04599b-t1.tif where ε1(ω) and ε2(ω) are frequency dependent real and imaginary parts of dielectric function, ω is photon frequency, μ0 is the permeability of free space.36 The real part of the dielectric function ε1(ω) can be evaluated from the imaginary part ε2(ω) by the famous Kramers–Kronig relationship.37 Direct optical band gap of the samples was obtained from the equation (αhν)n = A(Eopt), where A is a constant and n denotes the transition type as follows: n = 2 for direct allowed, 2/3 for direct forbidden, 1/2 for indirect allowed and 1/3 for indirect forbidden transitions.38 By extrapolating the linear proportion of the (αhν)n vs. hν plot to (αhν)n = 0 the optical band gap of the samples was calculated using Tauc plot.39

2.4 Photocatalytic performance

The photocatalytic performance of BFO bulk material and hydrothermally prepared nanoparticles at different reaction temperatures were subject to evaluation by photodegradation of rhodamine B (RhB)40 under illumination of visible light in aqueous solutions using a 500 W Xe lamp as a solar simulator accompanied with a visible cutoff filter (λ ≥ 420 nm). Beginning with a concentration of 15 mg L−1 of RhB, 80 mg of catalyst was later added to the solution in a quartz glass reactor for each experiment. Before illumination, the mixture was magnetically stirred in the dark for 1 hour for achieving the equilibrium between adsorption and desorption processes. After sufficient agitation, 4 ml of mixture was taken followed by centrifugation at 5000 rpm for 10 min so that the catalyst powders are removed. The concentration of RhB was then estimated from the measurement of the maximum absorbance at 553 nm with a UV-visible spectrophotometer. Testing for stability, the remaining photocatalyst powders in suspension were separated by centrifugation after photocatalytic degradation of RhB and distilled water was used to wash them to remove the residual RhB. Prior to using them in another photocatalytic reaction, they were further dried. The same procedure was followed three times. For comparison commercially available Degussa P25 titania nanoparticles were used to perform dye degradation experiment under the same experimental conditions.

2.5 Hydrogen generation

A photocatalytic hydrogen generation experiment has been performed in a slurry-type photochemical reactor. In a typical experiment, 20 mg of catalyst particles is measured and initiated in the reaction container with 30 ml water. Magnetic stirring is applied to mix the solution while purging the system with argon gas for 30 min to ensure an atmosphere, necessarily inert in nature as required for the splitting process. A 500 W xenon lamp was used for photoillumination. The gas was collected when each of the experiments ended and scrutinized in the gas chromatography (GC) device that is equipped with a thermal conductivity detector (TCD) and a gas analyzer for identifying the gas components. The GC programming, set up with a reverse polarization, made the hydrogen peaks occur in an upwards direction so that we can make a comparative analysis of the peak intensities of the different gases that were produced. The hydrogen evolution test was also performed for commercially available Degussa P25 titania nanoparticles under the same experimental conditions.

3 Results and discussions

3.1 Structural characterization

Crystal structure analysis. Fig. 1 shows the Rietveld refined XRD patterns of BFO nanoparticles synthesized by hydrothermal process at reaction temperatures 200 °C, 180 °C, 160 °C, 140 °C and 120 °C with the peaks indexed on the basis of rhombohedral structure (JCPDS File no. 71-2494). For the comparison, XRD pattern of BFO bulk polycrystalline sample prepared via conventional solid state reaction is also depicted in Fig. 1(a). Rietveld refinement was performed with the FULLPROF package.41 The structural variables and constituent phases (in wt%) calculated from the Rietveld refined XRD spectra of the synthesized materials have been provided in ESI Table 1.42 The small values of Rwp and Rp shown in ESI Table 142 indicate very good fit for hydrothermally prepared BFO nanoparticles to the rhombohedral structure. Reproduction of all the observed reflections can be performed from this structural model. Calculated lattice parameters (a and c) have been listed in Table 1 for all the major phases.
image file: c8ra04599b-f1.tif
Fig. 1 Rietveld plots of XRD patterns of (a) BFO bulk material synthesized by solid state reaction technique and hydrothermally prepared nanoparticles at reaction temperatures (b) 200 °C (c) 180 °C (d) 160 °C (e) 140 °C (f) 120 °C.
Table 1 Structural parameters determined from XRD spectra
Sample a = b (Å) c (Å) Volume3 (Å)3 Bond angle Fe–O–Fe (°) FeO6 tilt angle (ω in °)
BFO bulk 5.5775(1) 13.8663(1) 373.577 160.8753 10.310
BFO (200 °C) 5.5743(1) 13.8612(3) 373.003 158.6353 10.682
BFO (180 °C) 5.5761(1) 13.8634(3) 373.314 158.3842 10.807
BFO (160 °C) 5.5758(1) 13.8656(4) 373.327 152.8377 15.857


As was mentioned, the major phase of the synthesized materials is observed to be of rhombohedral crystal structure belonging to space group R3c. However, some secondary impurity phases are present for both bulk polycrystalline material and hydrothermally prepared nanoparticles at reaction temperatures 140 °C and 120 °C. For nanoparticles prepared at hydrothermal reaction temperatures 200 °C to 160 °C no obvious impurity phase (like Fe2O3, Fe3O4, Bi2Fe4O9 etc.) has been determined to the precision limit of XRD. Moreover, it is seen that for hydrothermal reaction temperature up to 160 °C, the nanoparticles (Fig. 1(b–d)) present a single-phase structure. For a further decrease of reaction temperature to 140 °C and 120 °C a structural transition to sillenite type Bi12.5Fe0.5O19.5 (Fig. 1(e and f)) phase is formed. Thus, the structural scrutiny clearly indicates that the minimal reaction temperature for obtaining perovskite type pure BFO phase is 160 °C. Therefore, we have carried out further characterization for nanoparticles prepared hydrothermally at reaction temperatures of 200–160 °C.

From the refinements of the XRD patterns, the Fe–O–Fe bond angle and FeO6 octahedral tilt angle ω are recapitulated in Table 1. The Fe–O–Fe bond angle of BFO bulk material and nanoparticles prepared at 200 °C, 180 °C and 160 °C reaction temperatures are 160.8753°, 158.6353 °C, 158.3842°, 152.8377°, respectively as shown in Table 1. The average Fe–O–Fe bond angle is maximum for bulk BFO material, however, a monotonic decrease of the average Fe–O–Fe angle from 158.6353 °C to 152.8377° is observed with decrease of hydrothermal reaction temperatures. Correspondingly, we observed an increase of the FeO6 octahedral tilt angle (ω) with the decrease of reaction temperatures. The alterations in the Fe–O–Fe bond angle and FeO6 octahedral tilt angle play role to modify the magnetic behavior of the synthesized nanoparticles.

Morphology analysis. The morphology of the surface and the size of the fabricated particles were analyzed by using FESEM imaging. The surface morphology and their corresponding histograms of bulk BFO sample produced by solid state reaction technique and BFO materials synthesized by hydrothermal method at 200 °C, 180 °C and 160 °C reaction temperatures are shown in Fig. 2. According to Fig. 2(a) and corresponding histogram Fig. 2(b), the average grain size of bulk BFO material is around 1 μm. The size of the bulk BiFeO3 was also determined from the XRD pattern (maximum intensity peak) using Scherrer equation and found to be around 600 nm which is comparable to the value obtained from FESEM image (Fig. 2(a and b)). FESEM images in Fig. 2(c and d) show BFO materials synthesized for the reaction temperatures 200 °C, and 180 °C, respectively. Fig. 2(e and f) depicts the BFO nanoparticles synthesized at 160 °C reaction temperature and their corresponding histogram for size distribution.
image file: c8ra04599b-f2.tif
Fig. 2 FESEM images of surface morphology of (a) BFO bulk material synthesized by solid state reaction technique and (b) corresponding histogram. Hydrothermally prepared nanoparticles at reaction temperatures (c) 200 °C (d) 180 °C, respectively. The nanoparticles and their corresponding histogram prepared at hydrothermal reaction temperature 160 °C are depicted in (e) and (f), respectively.

The electronic micrographs obtained by FESEM, Fig. 2(c and d), show the particles are prone to get interconnected with one another and aggregating to larger particles at higher reaction temperatures i.e. at 200 °C and 180 °C. However, for a comparatively lower reaction temperature of 160 °C, spherical and well dispersed BFO nanoparticles, Fig. 2(e and f) with sizes ranging from 20 nm to 30 nm is formed. Our investigation demonstrates that the morphology of the synthesized BiFeO3 materials changed from agglomerations to regular spherical shape with a narrow distribution of size when the reaction temperature is reduced from 200 °C to 160 °C. Previous investigation also reported such a change in morphology of BFO nanoparticles by varying the concentration of KOH for a fixed hydrothermal reaction temperature of 200 °C.43 We think, from energy consumption point of view it is much more desirable to control the surface morphology at a lower hydrothermal reaction temperature of 160 °C under a fixed concentration of KOH. Moreover, Bi is highly volatile and such a low processing temperature prevents reactants from getting volatilized during the formation of BFO powders and minimize the amount of impurities as was mentioned earlier.

During the hydrothermal preparation of BFO powders, the size of the final products depends on two mutually competitive processes: crystal nucleation and crystal growth.44 Provided the rate of crystal nucleation is greater than that of growth, then the product particle size becomes smaller. We expect that in our experiment with the decrease of reaction temperature to 160 °C, the growth rate was decreased, however, nucleation rate was increased and consequently the average size of the particles was significantly reduced. The smaller particle size may provide an increased surface area to volume ratio and substantial adsorption capacity, that is required to obtain a high photocatalytic performance.

X-ray photoelectron spectroscopic analysis. The XRD analysis and FESEM imaging confirmed that single phase, well crystalline BFO nanoparticles formed at 160 °C reaction temperature may meet the demand of practical applications. Therefore, X-ray photoelectron spectroscopy was carried out to further identify the chemical composition of BFO 160 nanoparticles which were prepared at hydrothermal reaction temperature 160 °C. Fig. 3 shows the typical full survey of XPS spectrum of BFO 160 nanoparticles. Observing the survey spectrum, aside from the weak peak of C 1s, only O, Fe, and Bi core levels were detected, indicating that the resulting product is highly pure. Fig. 3(b–d) shows the high resolution XPS spectra of the Bi 4f, Fe 2p and O 1s core levels for the BFO 160 nanoparticles, respectively. The core level XPS spectrum of Bi can be distinguished by two Gaussian peaks at 4 f7/2 and 4 f5/2 corresponding to the binding energy of 157.64 eV and 162.93 eV, respectively. The spin–orbit splitting energy of the Bi 4f is 5.3 eV.45,46 Fig. 3(c) shows a high resolution of XPS measurements for Fe contents. Two main peaks: one at 710.9 eV and another at 724.7 eV have been assigned to corresponding states of Fe 2p3/2 and 2p1/2 with the energy for spin–orbit splitting being 13.35 eV for Fe 2p.45 For a better insight of the chemical composition we have scrutinized the O 1s peak of BFO 160 nanoparticles (Fig. 3(d)) and bulk BiFeO3 materials Fig. 3(e). The uniformly single XPS peak of O 1s (530.29 eV) demonstrated that the BiFeO3 nanoparticles synthesized at 160 °C hydrothermal reaction temperature prepared in this investigation is indeed a compound of single-phase. The XPS spectrum of O 1s core level for bulk BiFeO3 materials, as shown in Fig. 3(e), can be de-convoluted into two symmetric Gaussian peaks. The lower binding energy peak at 529.8 eV corresponds to the O 1s core spectrum, while the higher binding energy peak is related to the oxygen vacancy in the bulk BFO sample.
image file: c8ra04599b-f3.tif
Fig. 3 XPS spectra of the as-synthesized BFO 160 nanopowders (a) a typical XPS survey spectrum, (b–d) high-resolution XPS core spectra of Bi 4f, Fe 2p, and O 1s, respectively. (e) XPS spectra of O 1s of BFO bulk materials.

3.2 Magnetic characterization

The field dependent magnetic hysteresis loops (MH) of bulk BFO material and hydrothermally synthesized nanoparticles are investigated at room temperature with an applied magnetic field of up to ±15 kOe. In Fig. 4, the obtained magnetization for bulk BFO prepared by solid state reaction technique changes linearly with magnetic field which demonstrates its antiferromagnetic nature.47,48 However, the magnetic behavior of BFO nanoparticles varies depending on hydrothermal reaction temperatures. We have calculated the remanent magnetization (Mr) of the synthesized samples from the MH hysteresis loops.49,50 The maximum magnetization (Ms) at an applied magnetic field of 13 kOe is also calculated from the hysteresis loops. Both Mr and Ms are higher for BFO nanoparticles prepared at 160 °C hydrothermal reaction temperature. In particular at 13 kOe applied magnetic field, the Ms value is 11.3 emu g−1 which is exceptionally high compared to the values reported in literature.51,52 In investigation,51 BFO nanoparticles with a particle size of 14 nm were prepared using sol–gel method for annealing temperature of 400 °C and the obtained Ms was 1.55 emu g−1 at 50 kOe. The observed Ms was 1.4 emu g−1 at 70 kOe for 18 nm BFO nanoparticles fabricated by sol–gel method with annealing temperature 425 °C.52 In our investigation, such a remarkable high value of magnetization (11.3 emu g−1) of the hydrothermally synthesized nanoparticles at reaction temperature 160 °C demands an extensive investigation of the magnetic behavior of this material.
image file: c8ra04599b-f4.tif
Fig. 4 The room temperature MH hysteresis loops of BFO bulk material synthesized by solid state reaction technique and hydrothermally prepared nanoparticles at reaction temperatures 200 °C, 180 °C and 160 °C.

The rationale behind improved magnetization can be imputed to several factors, such as: (i) the Rietveld refinement of XRD data (Table 1) clearly reveals that the Fe–O–Fe bond angle is minimum for nanoparticles with average size 20 nm produced at hydrothermal reaction temperature 160 °C. Such a decrement in Fe–O–Fe bond angle is crucial for developing ferromagnetism due to the strengthening of magnetic interaction caused by decreased Fe–O–Fe bond angle. This is consistent with previous investigations which reported that ferromagnetism can be realized in BFO by tuning Fe–O–Fe bond angle with reduced particle size.53,54 (ii) At room temperature, magnetization in G-type antiferromagnetic bulk BFO is subdued along with a spin helical ordering structure showing a periodicity of 62 nm. Compared to bulk materials, in the case of phase pure nanoparticles, the periodic spiral-regulated spin structure can be modified with the decrease in size of particles, and hence magnetization increases. (iii) The enhanced ferromagnetism in BFO nanoparticles with average particle 20 nm may be due to the reduced size of the phase pure nanoparticles. With decrease in particle size, the surface-to-volume ratio is enhanced and hence the surface spins contribute more to the arrant magnetic moment of the particle.23,49,51,52

3.3 Electric characterization

To further confirm the multiferroicity of hydrothermally prepared BFO 160 nanoparticles, PE hysteresis loops were investigated. Prior to conducting PE hysteresis, the leakage current density (J) versus electric field (E) measurements were carried out.

From Fig. 5(a), it can be implied that the leakage current density of the hydrothermally synthesized BFO 160 nanoparticles is smaller compared to that of the bulk. Impurity phases along with oxygen vacancies contribute to the high leakage current of bulk material.52,55 Previous demonstration from Fig. 1(d) for BFO 160 nanoparticles indicate inhibition of impurity phases. Furthermore, Fig. 3 shows that in BFO 160 nanoparticles, we observed only O 1s core spectrum, and obviously no oxygen vacancy related defects. Therefore, we think that the oxygen vacancies, principally induced by volatilized Bi3+ ion in the bulk material, were suppressed in BFO 160 nanoparticles and consequently the density of leakage current was reduced.


image file: c8ra04599b-f5.tif
Fig. 5 (a) Leakage current density of BFO bulk material and nanoparticles prepared at 160 °C hydrothermal reaction temperature. The polarization vs. electric field (PE) hysteresis loops of (b) BFO bulk material and (c) nanoparticles prepared at 160 °C hydrothermal reaction temperature.

Fig. 5(b and c) shows the polarization of ferroelectric hysteresis loops of (b) bulk BFO and (c) BFO 160 nanoparticles measured for varying electric fields. Driving frequency maintained at 50 Hz, continuously increasing electric field resulted in the increase of remanent polarization as stronger electric field with its higher level of driving power contributed to the reversal of ferroelectric domains.56

Freely movable charges are expected to contribute more to the electrical hysteresis loop for bulk BFO. Thus, the bulk BFO material shows a round shaped PE loop as observed in Fig. 5(b) owing to high leakage current which is evident from Fig. 5(a). For BFO 160 nanoparticles, the contribution of the dynamic charges to the polarization is reduced due to the decrease in rounded shapes of the loops. Furthermore, the PE loops of BFO nanoparticles tend to become increasingly typical which can be associated with the reduction in leakage current density57 and decreased space charge defect58 compared to that of bulk material. Thus, the measurement of electrical properties shows an improvement in ferroelectric behavior of BFO 160 nanoparticles. While comparing the PE loops between BFO bulk and BFO 160 nanoparticles, Fig. 5(b and c) also demonstrate that the significantly improved breakdown voltage up to 100 kV cm−1 for BFO 160 nanoparticles compared to 10 kV cm−1 for bulk material.

3.4 Optical characterization

Photocatalytic performance of a material depends on its ability to effectively absorb visible light. Optical band gap signifies the minimum energy of the photons that a material can absorb to generate electron–hole pairs via interband transition. To determine the optical band gap, the diffuse reflectance spectra of the synthesized materials were obtained from UV-vis spectrophotometric measurements. Determining F(R), a parameter proportional to the absorption coefficient, from the diffuse reflectance value using Kubelka–Munk function, we can have an estimate of the optical band gap,59
 
image file: c8ra04599b-t2.tif(1)

The band gap of the materials can be calculated by forming the Tauc plot using the following equation,59

 
F(R) × = A(Eg)n, (2)
where, , A, and Eg denote the energy of photons, constant of proportionality, and optical band gap, respectively. n is a number that takes the value of 1/2 and 2 for direct and indirect transitions, respectively. Since, BFO is widely regarded as a material with direct band gap, we have considered n = 1/2 and obtained the Tauc plots accordingly as shown in Fig. 6.


image file: c8ra04599b-f6.tif
Fig. 6 Tauc plots for band gap estimation of BFO bulk material synthesized by solid state reaction technique and hydrothermally prepared nanoparticles at reaction temperatures 200 °C, 180 °C and 160 °C.

Fig. 6 displays [F(R) × hv]2 vs. hv curves for optical band gap calculation of BFO bulk materials and nanoparticles hydrothermally synthesized at different reaction temperatures. Extrapolating the linear region of the curve to the energy axis, we can determine the band gap. Optical band gap for bulk BFO material is found to be 2.1 eV. For hydrothermally prepared nanoparticles at reactions temperatures 200 °C, 180 °C and 160 °C, the direct band gaps are 2.05 eV, 2.11 eV and 2.1 eV, respectively. This energy band gap is consistent with value reported in ref. 20 and 60. However, in those investigations, nanoparticles were produced at considerably higher annealing temperatures. The small band gap exhibited by synthesized BFO bulk and nanoparticles indicates their potential as good photocatalysts since they are capable of absorbing visible range photons effectively. However, all the synthesized materials have almost equal band gaps and hence, superiority of a particular sample in photocatalytic applications cannot attributed solely to its band gap. Rather, there are other factors which will also play important roles in determining the efficiency of a material as photocatalyst such as particle size, surface morphology, phase purity, ability to suppress electron–hole recombination etc.

Theoretical calculation of band gap. BFO bulk and BFO 160 nanoparticles were subject to First-principles calculation with a view to comparing the experimentally obtained values of band gap to the theoretically calculated ones. While standard DFT methods are widely in use for such calculations, experimentally obtained outcomes of BiFeO3 are more closely comparable to the DFT calculated values when Hubbard U parameter, a measure of effective on-site Coulomb interaction, is chosen carefully.61–65 Experimentally obtained crystallographic parameters were refined by Rietveld method and their geometry was optimized prior to using them for DFT calculations. PDOS, electronic band structure and optical absorption spectra of both BFO bulk and BFO 160 nanoparticles were obtained via DFT calculations using GGA-PBE functionals. While performing DFT calculations, U value was varied from 3.0 eV to 7.0 eV at 0.5 eV interval. DFT calculated absorption spectra closely match the experimentally obtained ones for U = 4.5 eV and therefore, further observations were carried out for this value of U. As we can observe from the PDOS spectra (Fig. 7(a and b)) of both BFO bulk and BFO 160, conduction band minima(CBM) is dominated by 3d orbital of Fe atoms and 2p orbital of oxygen atoms dominate the valence band maxima (VBM). We can infer from this observation that the electron transitions from VBM to CBM can be attributed to these two orbitals and there are no major d–d transitions involved. From the electronic band structures as shown in Fig. 7(c and d), VBM lies between Z and L point for BFO bulk and BFO 160 nanoparticles and hence the calculated direct band gap for both materials found to be 2.1 eV. Since, transition from 2p orbital of oxygen atoms to 3d orbitals of Fe atoms is allowed and direct, our use of n = 2 in the formation of Tauc plot from experimentally obtained absorption coefficients is justified. Fig. 7(e) shows the theoretical optical absorption coefficients of BFO bulk and BFO 160 obtained from our DFT calculation. These absorption spectra were transformed into Tauc plots as shown in Fig. 7(f) and tangents were drawn to the linear region of the plot. Extrapolating the tangent to the energy axis, optical band gap of the corresponding material was found from the energy axis intercept. As observed from Fig. 7(f), both BFO bulk and BFO 160 exhibit the same direct optical band gap of 2.1 eV. These theoretically calculated values are in excellent agreement with the ones experimentally determined (2.1 eV for both BFO bulk and BFO 160). With this agreement between theoretical and experimental calculation, we can conclude that there has been no significant change in the optical band gap for BFO bulk and nanoparticles.
image file: c8ra04599b-f7.tif
Fig. 7 DFT calculated PDOS spectra of (a) BFO bulk and (b) BFO 160; band structures of (c) BFO bulk and (d) BFO 160; DFT calculated absorption spectra of (e) BFO bulk and BFO 160; (f) plot of DFT calculated (αhν)2 vs. hν for BFO bulk and BFO 160.

3.5 Photocatalytic activity

The photocatalytic performance of the fabricated materials was studied extensively through degradation of the typical organic contaminant rhodamine-B (RhB) under visible light illumination66 at λ ≥ 420 nm. Fig. 8(a) shows how intensity of the absorbance peak of RhB for BFO 160 nanoparticles typically varies under visible-light irradiation. The absorbance peak corresponding to RhB decreases gradually with increasing time, implying that RhB has been decomposed by BFO. Due to the well known fact that RhB dye shows a general resistance to decomposition, the implication of the results is that the photocatalytic activity of BFO nanoparticles is quite efficient and hence indicates the promise as visible light photocatalysts for BFO nanoparticles.
image file: c8ra04599b-f8.tif
Fig. 8 (a) Absorption spectra of rhodamine B (RhB) under visible-light irradiation in the presence of BFO nanoparticles prepared at 160 °C hydrothermal reaction temperature. (b) Photocatalytic degradation of RhB as a function of the visible light irradiation time for blank sample, Degussa P25 titania, BFO bulk material and hydrothermally prepared nanoparticles at reaction temperatures 200 °C, 180 °C and 160 °C. (c) Pseudo-first order kinetics fitting data for the photodegradation of RhB. (d) Volume of H2 evolution as a function of irradiation time during the photocatalytic splitting of water. (e) Schematic illustration of RhB degradation and water splitting mechanism using BFO nanoparticles as catalysts under visible light irradiation.

For evaluating the efficiency of degradation of RhB, the maximum intensity ratio C/C0 is plotted in Fig. 8(b), in which C0 and C are the maximum initial intensity (0 h) and maximum intensity at a specific time (1–4 h) respectively for the absorption spectra of RhB under stimulated sunlight irradiation. A blank test is evaluated for RhB (Fig. 8(b)) and it exhibits a negligible degradation efficiency which clearly shows a nominal self-degradation potential of RhB. For example, after 4 hours of irradiation without BFO materials, RhB was degraded by less than 3%, whereas the bulk BFO photocatalyst could decompose 56% of RhB after 4 h irradiation. Notably, when hydrothermally prepared nanoparticles were used as photocatalysts, the degradation efficiency was increased to 59% and 61% for nanoparticles prepared at 200 °C and 180 °C hydrothermal reaction temperatures. Interestingly, RhB photodegradation attains a significant improvement in efficiency to 79% for BFO 160 nanoparticles which were prepared at 160 °C reaction temperature.

In a similar investigation BiFeO3 particles with the size of 100-150 nm were synthesized at the temperature as low as 120 °C via a urea-assisted hydrothermal process.67 Their photocatalytic activity was evaluated by the degradation of RhB in aqueous solution under visible-light irradiation using a 500 W Xe lamp with a cutoff filter (λ ≥ 420 nm). The condition for photocatalytic experiment was same as that of our experiment. Moreover, the optical band gap of the particles was 2.1 eV which is also consistent with that of the nanoparticles synthesized in the present investigation. However, in ref. 67 it was observed that only 40% of RhB was decomposed after 4 h visible-light irradiation. Though the band gap of the BFO particles synthesized both in ref. 67 and in our investigation was same, however, the photocatalytic dye degradation is much higher while BFO 160 nanoparticles are used as photocatalysts. In another recent investigation,68 the photocatalytic activity of BFO nanoparticles with a particle size of 40 nm was evaluated by photocatalytic decomposition of RhB in aqueous solution under visible light irradiation. It is observed that the pure BFO photocatalyst could decompose 22.3% of RhB after 270 min visible light irradiation.

The photodegradation of BFO 160 nanoparticles is much higher compared to that of other materials in particular commercially available Degussa P25 titania nanoparticles and BFO bulk materials. For comparison, the photodegradation efficiency of BFO 140 and BFO 120 materials was also evaluated under the same experimental condition. The degradation efficiency was found to 53% and 42% for using BFO 140 and BFO 120 particles, respectively. Our investigation clearly demonstrated that the photocatalytic activity of BFO 160 nanoparticles for photocatalytic decomposition of RhB in aqueous solution under visible light irradiation is higher compared than that of other materials under investigation. The enhanced photodegradation efficiency of BFO 160 nanoparticles might have resulted from the reduced particle size with excellent crystallinity. Looking at the SEM image, Fig. 2(e and f), significantly greater surface area of the BFO 160 nanoparticles can be attributed to the higher photodegradation efficiency. It should also be noted that compared to commercially available photocatalyst TiO2, that responds only to UV irradiation, BFO nanoparticles are more advantageous as they make use of the visible portion of the spectrum.

For quantitative investigation of the rate of degradation, the experimental data were fitted adapting a first-order model as elucidated by the following equation, ln(C0/C) = kt,69 where C0 and C denote the respective concentrations of RhB at distinct irradiation times of t0 and t, k is the first-order rate constant and can be regarded as a basic kinetic parameter for a number of different photocatalysts. For the photodegradation of RhB, the pseudo-first order kinetics fitting data has been shown in Fig. 8(c). The corresponding reaction rate constant (k) values were calculated to be 7.66 × 10−3, 2.27 × 10−1, 2.47 × 10−1, 2.72 × 10−1, and 3.23 × 10−1 min−1 for the blank sample, bulk BFO, hydrothermally prepared nanoparticles at reaction temperatures 200 °C, 180 °C and 160 °C, respectively (Table 2). Among them, the BFO 160 nanoparticles exhibited the highest k value, which is 1.42 times higher than that of bulk BFO. Notably, BFO 160 nanoparticles were subject to recyclability test under the same test conditions. The test result indicates excellent stability of these nanoparticles after 4 cycles.

Table 2 Calculated band gap energy (Eg), rate constant (k), and degradation efficiency of BFO bulk and hydrothermally prepared nanoparticles
Sample Eg in eV Rate constant (k) × 10−1 Degradation (%) after 4 h
BFO bulk 2.1 2.27 56
BFO (200 °C) 2.05 2.47 59
BFO (180 °C) 2.11 2.72 61
BFO (160 °C) 2.1 3.23 71


3.6 Photocatalytic hydrogen production

Now, we have examined the potential of BFO materials for hydrogen generation via water splitting under visible light irradiation.4 No hydrogen evolution could be detected when a blank experiment without any photocatalyst was performed in dark conditions. Fig. 8(d) shows the hydrogen evolution rate of BFO bulk material as well as hydrothermally prepared BFO 160 nanoparticles in ml H2 per g catalyst plotted against visible light irradiation time in hours (h). For comparison, we have inserted in Fig. 8(d) the hydrogen production rate of commercially available Degussa P25 titania nanoparticles. The outcome of our investigation demonstrates that BFO 160 nanoparticles prepared hydrothermally at reaction temperatures 160 °C generate nearly two times hydrogen compared to that of bulk BFO material after 4 h of illumination. Compared to commercially available TiO2, the production rate of BFO 160 nanoparticles is more than double after 4 h of illumination. In a separate investigation,13 BFO nanoparticles as photocatalyst were also used for solar hydrogen generation from water and the production rate after 4 h illumination is equivalent with that of our investigation. But here the noteworthy point is that, in ref. 13, the nanoparticles of size 50–60 nm were produced at comparatively high temperature sol–gel process. Particularly the nanoparticles used for hydrogen production in ref. 13 was subject to annealing at 600 °C for 2 hours in N2 atmosphere. Whereas in the present investigation a facile, low cost hydrothermal process has been used for fabrication of nanoparticles and the reaction temperature was only 160 °C which ensures the less energy consumption.

3.7 Photocatalytic mechanism

The photocatalytic performance under visible light irradiation depends on a number of parameters cooperating with each other ultimately ameliorating the photocatalytic performance. Fig. 8(e) schematically illustrates degradation of RhB and water splitting mechanism using BFO nanoparticles under visible light irradiation.5

Photocatalysis is an electrochemical process that involves the transfer of the photogenerated electrons and holes between a semiconductor and an electrolyte. The semiconductor in this investigation is BFO, and the electrolyte is the RhB solution. When the BFO nanoparticles are dispersed in the RhB solution under visible light irradiation, the electrons in their valence band are excited to the conduction band by absorbing the photons of the visible light. This transition creates holes in the valence band of BFO. On the other hand, an electrolyte in equilibrium has one or more redox couples with specific redox potentials. If the potential of the photogenerated electrons in a semiconductor is lower than any of these redox couples, the electrons will flow into the electrolyte to perform reduction of that couple. Similarly, if the potential of the photogenerated holes of the semiconductor is higher than a redox couple, the holes will flow into the electrolyte to oxidize it. The reduced and oxidized species can initiate further reactions that are responsible for degrading the electrolyte. Besides determining the potentials of the conduction band minima (CBM) and valence band maxima (VBM) of BFO, we need to investigate the redox potentials of the redox couples that dictate the degradation of RhB to learn about the photocatalytic mechanism behind the degradation of RhB. The potentials of CBM and VBM of BFO have been determined to be 0.3 V and 2.4 V respectively using the absolute electronegativity theory.70,71

The degradation of RhB dye depends primarily on two critical redox reactions. First, the photogenerated electron can react with the surface adsorbed O2 (redox potential: −0.16 V vs. NHE) to form O2, which will further react with RhB to cause degradation.72,73 Second, the photogenerated holes can react with the OH ionized from the water molecules to produce ·OH (redox potential: 2.38 V vs. NHE). This ·OH can further oxidize the RhB molecules. Therefore, a photocatalyst needs to possess a CBM < −0.16 V to drive the first reaction and VBM > 2.38 V to drive the second one efficiently. Therefore, only the photogenerated holes are capable of performing the second reaction. However, when photons with energy higher than 2.56 eV are incident on BFO nanoparticles, the electrons in their valence band can be excited to the higher states of the conduction band where their potential can be more negative than −0.16 V. These photogenerated electrons will be able to perform the first reaction. Since BFO can absorb visible light photons with energies higher than 2.56 eV, both these reactions can contribute to the degradation of RhB.74 In addition, RhB self-photoexcitation may also play a role in assisting the photodegradation process. The RhB molecules can absorb the visible range photons to reach an excited state of a potential of −1.09 V.75 Since the potential of electrons in this state is more negative than the CBM of BFO nanoparticles, the electrons of the photoexcited state will be transferred to the conduction band of BFO. However, these electrons cannot participate in the photocatalytic degradation process as they cannot reduce O2 to O2. Consequently, these electrons will be accumulated in the conduction band of BFO and the transfer of electrons from the photoexcited state of RhB will stop when both states reach the same potential. Hence, the self-photoexcitation of RhB may not have a significant effect on the photocatalytic degradation of RhB.

It is well known that the size of the particles and surface area significantly effect the enhancement of the photocatalytic degradation. In our investigation, the degradation of RhB with BFO 160 nanoparticles is considerably greater than that of bulk BFO owing to their smaller size and higher surface area. The band gap is another important parameter as the low band gap of photocatalysts might increase the photocatalytic activities.76 We observed that the band gap is almost same (2.1 eV) for nanoparticles prepared at all hydrothermal reaction temperatures as well as the bulk BFO. While sunlight hits the photocatalyst, photons possessing greater energy than the optical band gap of the photocatalyst cause stronger light absorption. The estimated band gap 2.1 eV for both BFO bulk and nanoparticles implied that light with λ less than 590 nm could be absorbed by e to jump from valence band (VB) to conduction band (CB) which covers a broad region of the solar energy spectrum. With all the materials under scrutiny having almost equal band gap, the other factors prove to be more important for achieving higher photocatalytic efficiency of BFO 160 nanoparticles rather than band gap itself.

It was mentioned already in introduction section that, BFO is an well known multiferroic materials. It is evident that the ferroelectric property of a material enhances its ability to decolorize rhodamine-B, a typical dye molecule, while irradiated by solar light.77 Ferroelectric materials have a spontaneous polarization that is caused by the non-centrosymmetry of the crystal structure. As nanoparticles are more strained than their bulk counterparts, their crystal structures deviate from the bulk structure and give rise to even greater non-centrosymmetry for BFO. This essentially increases the magnitude of spontaneous polarization of BFO nanoparticles, especially for BFO 160 with smallest particle sizes as evident from our experimental values. The BFO 160 nanoparticles, assumed to be creating electrical field in the surrounding medium, improves redox reactions along with the adsorption of dye molecules, especially polar molecules such as water on the photocatalyst surface. This adsorption helps the redox reactions to commence easily as the carrier transport is now relatively easier. Furthermore, it is anticipated that ferroelectrics can create channels to transfer the charge carriers to the surface of photocatalyst and significantly reduce the recombination probabilities as the photogenerated electron–hole pairs are driven to opposite directions by the electric field they possess.

4 Conclusions

We have synthesized single-phase, well crystalline BiFeO3 nanoparticles with favorable morphology using a facile, low cost hydrothermal process at reaction temperature as low as 160 °C. The experimentally observed band gap (2.1 eV) was almost equal for both bulk and all nanoparticles prepared at different reaction temperatures and was well consistent with value obtained from the first principles calculation. However, the BFO 160 nanoparticles prepared at temperature 160 °C demonstrated much higher photocatalytic activity compared to the photocatalytic performance showed by bulk BFO and other nanoparticles. The enhanced photocatalytic activities of BFO 160 nanoparticles may be associated with their crystallinity, phase purity, excellent morphology, higher surface to volume ratio, and the efficient separation and migration of photogenerated charge carriers. As efficient photocatalyst, the synthesized BFO 160 nanoparticles generated more than two times of solar hydrogen via water splitting compared to that produced by bulk BiFeO3 as well as commercially available Degussa P25 titania. The outcome of this investigation also demonstrated an improved multiferroic properties of technologically important BiFeO3 nanoparticles prepared at temperature as low as 160 °C which is cost effective with less energy consumption. BiFeO3 nano-structured particles prepared through this investigation have shown a great promise in enhancing the production of solar H2, a carbon free fuel, using two important renewable sources: water and solar energy.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This research work was financially supported by Ministry of Education, Government of Bangladesh (Grant No. PS 14267) and also by HEQEP sub-project CP-6038. The computational facility was provided by IICT, BUET.

Notes and references

  1. R. Guo, L. Fang, W. Dong, F. Zheng and M. Shen, J. Phys. Chem. C, 2010, 114, 21390–21396 CrossRef .
  2. J. Shi and L. Guo, Prog. Nat. Sci.: Mater. Int., 2012, 22, 592 CrossRef .
  3. B. Wang, C. Li, D. Hirabayashi and K. Suzuki, Int. J. Hydrogen Energy, 2010, 35, 3306–3312 CrossRef .
  4. K.-Q. Lu, X. Xin, N. Zhang, Zi-R. Tang and Yi-J. Xu, J. Mater. Chem. A, 2018, 6, 4590–4604 RSC .
  5. Y. Lan, H. Chuang, M.-Q. Yanga and Y.-J. Xu, Int. Rev. Phys. Chem., 2016, 35(1), 1–36 Search PubMed .
  6. N. Zhang, M.-Q. Yang, S. Liu, Y. Sun and Yi-J. Xu, Chem. Rev., 2015, 115, 10307–10377 CrossRef PubMed .
  7. F. Wang, T. Shen, Z. Fu, Y. Lu and C. Chen, Nanotechnology, 2017, 29, 035702 CrossRef PubMed .
  8. A. Fujishima and K. Honda, Nature, 1972, 238, 37–38 CrossRef PubMed .
  9. A. A. Nada, M. H. Barakat, H. A. Hamed, N. R. Mohamed and T. N. Veziroglu, Int. J. Hydrogen Energy, 2005, 30, 687–691 CrossRef .
  10. Y. Liu, L. Xie, Y. Li, R. Yang, J. Qu, Y. Li and X. Li, J. Power Sources, 2008, 183, 701 CrossRef .
  11. D. Jian, P.-X. Gao, W. Cai, B. S. Allimi, S. Pamir Alpay, Y. Ding, Z. L. Wang and C. Brooks, J. Mater. Chem., 2009, 19, 970 RSC .
  12. H. Park, W. Choi and M. R. Hoffmann, J. Mater. Chem., 2008, 18, 2379 RSC .
  13. J. Deng, S. Banerjee, S. K. Mohapatra, Y. R. Smith and M. Misra, J. Fundam. Renewable Energy Appl., 2011, 1, 10 Search PubMed .
  14. T. Choi, S. Lee, Y. J. Choi, V. Kiryukhin and S.-W. Cheong, Science, 2009, 324, 63–66 CrossRef PubMed .
  15. A. B. Murphy, P. R. F. Barnes, L. K. Randeniya, I. C. Plumb, I. E. Grey, M. D. Horne and J. A. Glasscock, Int. J. Hydrogen Energy, 2006, 31, 1999 CrossRef .
  16. F. E. Osterloh, Chem. Mater., 2008, 20, 35–54 CrossRef .
  17. K. Rajeshwar, R. McConnell and S. Licht, Solar Hydrogen Generation: Toward a Renewable Energy Future, Kluwer Academic, New York, 2008 Search PubMed .
  18. Y. Yang, I. C. Infante, B. Dkhil and L. Bellaiche, C. R. Phys., 2015, 16, 193 CrossRef .
  19. J. Schneider, M. Matsuoka, M. Takeuchi, J. Zhang, Y. Horiuchi, M. Anpo and D. W. Bahnemann, Chem. Rev., 2014, 114, 9919–9986 CrossRef PubMed .
  20. F. Gao, X. Y. Chen, K. B. Yin, S. Dong, Z. F. Ren, F. Yuan, T. Yu, Z. G. Zou and J. M. Liu, Adv. Mater., 2007, 19, 2889 CrossRef .
  21. C. C. Moo, N. J. Hong, C. In-Sun, A. Jae-Sul, H. K. Sun and K. J. Young, J. Am. Ceram. Soc., 2008, 91, 3753 CrossRef .
  22. G. Sushmita, D. Subrata, S. Amarnath and S. M. Himadri, J. Am. Ceram. Soc., 2005, 88, 1349 CrossRef .
  23. M. A. Basith, D. T. Ngo, A. Quader, M. A. Rahman, B. L. Sinha, B. Ahmmad, F. Hirose and K. Molhave, Nanoscale, 2014, 6, 14336 RSC .
  24. N. Das, R. Majumdar, A. Sen and H. S. Maiti, Mater. Lett., 2007, 61, 2100 CrossRef .
  25. S. Komarneni, V. C. Menon, Q. H. Li, R. Roy and F. Ainger, J. Am. Ceram. Soc., 1996, 79, 1409–1412 CrossRef .
  26. T. T. Carvalho and P. B. Tavares, Mater. Lett., 2008, 62, 3984 CrossRef .
  27. S. H. Han, K. S. Kim, H. G. Kim, H.-G. Lee, H.-W. Kang, J. S. Kim and C. I. Cheon, Ceram. Int., 2010, 36, 1365 CrossRef .
  28. S. Li, Y.-H. Lin, B.-P. Zhang, Y. Wang and C.-W. Nan, J. Phys. Chem. C, 2010, 114, 2903–2908 CrossRef .
  29. Y. Wang, G. Xu, Z. Ren, X. Wei, W. Weng, P. Du, G. Shen and G. Han, Ceram. Int., 2008, 34, 1569 CrossRef .
  30. M. A. Basith, O. Kurni, M. S. Alam, B. L. Sinha and B. Ahmmad, J. Appl. Phys., 2014, 115, 024102 CrossRef .
  31. S. S. Chowdhury, A. H. M. Kamal, R. Hossain, M. Hasan, M. F. Islam, B. Ahmmad and M. A. Basith, Ceram. Int., 2017, 43, 9191 CrossRef .
  32. R. G. Freitas, F. W. S. Lucas, M. A. Santanna, R. A. Mendes, A. J. Terezo, G. L. C. de Souza, L. H. Mascaro and E. C. Pereira, Phys. Chem. Chem. Phys., 2016, 18, 26885 RSC .
  33. J. Clark Stewart, D. Segall Matthew, J. Pickard Chris, J. Hasnip Phil, I. J. Probert Matt, K. Refson and C. Payne Mike, Z. Kristallogr. - Cryst. Mater., 2005, 220, 567 Search PubMed .
  34. B. Himmetoglu, A. Floris, S. Gironcoli and M. Cococcioni, Int. J. Quantum Chem., 2014, 114, 14–49 CrossRef .
  35. G. Kresse and D. Joubert, Phys. Rev. B, 1999, 59, 1758 CrossRef .
  36. M. Tamer, AIP Adv., 2016, 6, 065115 CrossRef .
  37. X. D. Zhang, M. L. Guo, W. X. Li and C. L. Liu, J. Appl. Phys., 2008, 103, 063721 CrossRef .
  38. N. Serpone, D. Lawless and R. Khairutdinov, J. Phys. Chem., 1995, 99, 16646–16654 CrossRef .
  39. N. Gao, C. Quan, Y. Ma, Y. Han, Z. Wu, W. Mao, J. Zhang, J. Yang, X. a Li and W. Huang, Phys. B: Condens. Matter, 2016, 481, 45 CrossRef .
  40. C. Regmi, D. Dhakal, T.-H. Kim, T. Yamaguchi and S. W. Lee, Nanotechnology, 2018, 29, 154001 CrossRef PubMed .
  41. J. Rodriguez-Carvajal, Fullprof: A Program for Rietveld Refinement and Pattern Matching Analysis, Abstract of the Satellite Meeting on Powder Diffraction of the XV Congress of the IUCr, Toulouse, France, 1990, p. 127 Search PubMed .
  42. ESI: Rietveld refined structural parameters and phases present (in wt%) obtained from XRD analysis.
  43. J.-P. Zhou, R.-L. Yang, R.-J. Xiao, X.-M. Chen and C.-Y. Deng, Mater. Res. Bull., 2012, 47, 3630–3636 CrossRef .
  44. S. Er-Wei, X. Chang-Tai, Z. Wei-Zhou, W. Bu-Guo and F. Chu-De, J. Am. Ceram. Soc., 1997, 80, 1567 Search PubMed .
  45. S. Han and C. S. Kim, J. Appl. Phys., 2013, 113, 17D92 Search PubMed .
  46. R. Das, S. Sharma and K. Mandal, J. Magn. Magn. Mater., 2016, 401, 129–137 CrossRef .
  47. J. T. Han, Y. H. Huang, X. J. Wu, C. L. Wu, W. We, B. Peng, W. Huang and J. B. Goodenough, Adv. Mater., 2006, 18, 2145 CrossRef .
  48. B. Ahammad, M. Z. Islam, A. Billah and M. A. Basith, J. Phys. D: Appl. Phys., 2016, 49, 095001 CrossRef .
  49. M. A. Basith, F. A. Khan, B. Ahmmad, S. Kubota, F. Hirose, D.-T. Ngo, Q.-H. Tran and K. Molhave, J. Appl. Phys., 2015, 118, 023901 CrossRef .
  50. B. Ahmmad, K. Kanomata, K. Koike, S. Kubota, H. Kato, F. Hirose, A. Billah, M. A. Jalil and M. A. Basith, J. Phys. D: Appl. Phys., 2016, 49, 265003 CrossRef .
  51. T.-J. Park, G. C. Papaefthymiou, A. J. Viescas, A. R. Moodenbaugh and S. S. Wong, Nano Lett., 2007, 7, 766–772 CrossRef PubMed .
  52. F. Huang, Z. Wang, X. Lu, J. Zhang, K. Min, W. Lin, R. Ti, T. Xu, J. He, C. Yue and J. Zhu, Sci. Rep., 2013, 3, 2907 CrossRef PubMed .
  53. P. Modak, D. Lahiri and S. M. Sharma, J. Phys. Chem. C, 2016, 120, 8411–8416 CrossRef .
  54. H. Zhang, W. Liu, P. Wu, X. Hai, M. Guo, X. Xi, J. Gao, X. Wang, F. Guo, X. Xu, C. Wang, G. Liu, W. Chu and S. Wang, Nanoscale, 2014, 6, 10831 RSC .
  55. A. R. Makhdoom, M. J. Akhtar, M. A. Rafiq and M. M. Hassan, Ceram. Int., 2012, 38, 3829–3834 CrossRef .
  56. M. S. Wu, Z. B. Huang, C. X. Han, S. L. Yuan, C. L. Lu and S. C. Xia, Solid State Commun., 2012, 152, 2142 CrossRef .
  57. H. Deng, M. Zhang, Z. Hu, Q. Xie, Q. Zhong, J. Wei and H. Yan, J. Alloys Compd., 2014, 582, 273 CrossRef .
  58. A. Mukherjee, S. Basu, P. K. Manna, S. M. Yusuf and M. Pal, J. Mater. Chem. C, 2014, 2, 5885–5891 RSC .
  59. M. Sakar, S. Balakumar, P. Saravanan and S. Bharathkumar, Nanoscale, 2015, 7, 10667–10679 RSC .
  60. R. Ahsan, M. Z. R. Khan and M. A. Basith, J. Nanophotonics, 2017, 11, 046016 Search PubMed .
  61. Y.-T. Peng, S.-T. Chiou, C.-H. Hsiao, C. H. Ouyang and C.-H. Tu, Sci. Rep., 2017, 7, 45164 CrossRef PubMed .
  62. J. K. Shenton, D. R. Bowler and W. L. Cheah, J. Phys.: Condens. Matter, 2017, 29, 445501 CrossRef PubMed .
  63. J. Mao, L. Cao, Z. Xiong, X. Wang, J. Zhou, Y. Li and W. Wu, J. Alloys Compd., 2017, 721, 638 CrossRef .
  64. M. Cebela, D. Zagorac, K. Batalovic, J. Radakovic, B. Stojadinovic, V. Spasojevic and R. Hercigonja, Ceram. Int., 2017, 43, 1256 CrossRef .
  65. N. S. A. Satar, A. W. Aziz, M. K. Yaakob, M. Z. A. Yahya, O. H. Hassan, T. I. T. Kudin and N. H. M. Kaus, J. Phys. Chem. C, 2016, 120, 26012 CrossRef .
  66. X. Ren, H. Yang, S. Gen, J. Zhou, T. Yang, X. Zhang, Z. Cheng and S. Sun, Nanoscale, 2016, 8, 752–756 RSC .
  67. J. Wei, C. Zhang and Z. Xu, Mater. Res. Bull., 2012, 47, 3513–3517 CrossRef .
  68. N. Zhang, D. Chen, F. Niu, S. Wang, L. Qin and Y. Huang, Sci. Rep., 2016, 6, 26467 CrossRef PubMed .
  69. S. Ma, R. Li, C. Lv, W. Xu and X. Gou, J. Hazard. Mater., 2011, 192, 730–740 CrossRef PubMed .
  70. A. H. Nethercot, Phys. Rev. Lett., 1974, 33, 1088–1091 CrossRef .
  71. M. Butler and D. Ginley, J. Mater. Sci., 1980, 15, 1–19 CrossRef .
  72. X. Ren, H. Yang, S. Gen, J. Zhou, T. Yang, X. Zhang, Z. Cheng and S. Sun, Nanoscale, 2016, 8, 752–756 RSC .
  73. R. Ahsan, A. Mitra, S. Omar, M. Z. Rahman Khan and M. A. Basith, RSC Adv., 2018, 8, 14258–14267 RSC .
  74. M. A. Basith, R. Ahsan, I. Zarin and M. A. Jalil, Sci. Rep., 2018, 8, 11090 CrossRef PubMed .
  75. L. Yuan, M.-Q. Yang and Y.-J. Xu, Nanoscale, 2014, 6, 6335–6345 RSC .
  76. S. Irfan, S. Rizwan, Y. Shen, L. Li, Asfandiyar, S. Butt and C.-W. Nan, Sci. Rep., 2017, 7, 42493 CrossRef PubMed .
  77. Y. Cui, J. Briscoe and S. Dunn, Chem. Mater., 2013, 25, 4215–4223 CrossRef .

Footnote

Electronic supplementary information (ESI) available. See DOI: 10.1039/c8ra04599b

This journal is © The Royal Society of Chemistry 2018