Lorena Alcaraz Romoa,
Ana López-Fernándeza,
Irene García-Díaza,
Paloma Fernándezb,
Ana Urbietab and
Félix A. López*a
aCentro Nacional de Investigaciones Metalúrgicas (CENIM-CSIC), Avda. Gregorio del Amo 8, 28040 Madrid, Spain. E-mail: f.lopez@csic.es; Fax: +34-915-347425; Tel: +34-915-538-900
bFacultad de Ciencias Físicas, Universidad Complutense de Madrid, Ciudad Universitaria, Plaza de las Ciencias, 28040 Madrid, Spain
First published on 28th September 2018
A series of Zn/Mn binary oxides with different molar ratios (1.4–11) were synthesized via co-precipitation from a solution obtained through the acidic (HCl) leaching of a black mass originating from the mechanical recycling of spent alkaline and Zn–C batteries. The oxides obtained were characterized by X-ray diffraction (XRD), Fourier-transform infrared spectroscopy (FTIR), X-ray photoelectron spectroscopy (XPS), and Raman spectroscopy. Magnetic properties of the samples were also investigated. The Raman spectroscopy results showed all the binary metallic oxides belong to the ZnxMn3−xO4 (0.25 ≤ x ≥ 1.75) type. All showed a spinel crystalline structure. The saturation magnetization decreases with the Zn/Mn molar ratio; a maximum of 13.19 emu g−1 was found for the molar ratio of 11 at the Curie temperature (25.5 K). XPS showed that all the synthesized compounds contained Mn2+, Mn3+ and Mn4+. Mn2+ was the most prominent at a molar ratio of 11, Mn3+ was most common at a molar ratio of 2, and Mn4+ at 1.4.
The main components of batteries are manganese dioxide (positive electrode), zinc (negative electrode), an electrolyte (KOH or ZnCl2 + NH4Cl), and the steel casing. These compounds and any other heavy metals they may contain (e.g., cadmium, mercury, lead, lithium) may seep out, negatively affecting the environment and human health.4–6 These dangers, plus the elevated costs associated with the adequate management of these spent products, make the recycling of batteries an attractive option.7
The techniques developed for processing spent batteries fall into three groups: mechanical separation, pyrometallurgical treatment, and hydrometallurgical treatment.8 Mechanical separation is commonly required before any further processing, especially hydrometallurgical processing. The aim is to separate the electrodes, steel casing and any plastic or paper components.9 Mechanical separation usually involves cutting/milling, magnetic separation, dimensional separation (screening), eddy current separation (ECS) employing Foucault currents, and the final milling of the particulate fraction.7 The result is a so-called 'black mass' (consisting largely of electrolytes, graphite, and oxides of zinc and manganese). Although pyrometallurgical treatment is the most commonly used method10,11 hydrometallurgical treatment is gaining attention given its low cost and more environmentally friendly nature.12
The hydrometallurgical treatment of spent battery black mass takes place in several stages: pre-treatment, acidic or alkaline leaching, and the recovery of the Zn and Mn via electrolysis, liquid–liquid extraction, or selective precipitation.13 The use of biological processes for this is also of interest since they are likely to be less environmentally harmful.14,15 Several hydrometallurgical processes have been patented for the industrial scale recovery of Mn and Zn from spent batteries, including the Bateaux,16 Recupyl17 and Revabat18 processes, among others.
Previous work performed by the present authors showed it is possible to obtain highly pure ZnO from black mass via leaching with ammoniacal ammonium carbonate.19,20 This ZnO has good luminescent properties and can be used in gas sensors.21
Ternary compounds of metallic oxides that contain transition metals of the AB2O4 type are currently a focus of research. In this context ZnO, doped with a certain amount of Mn, forms interesting spinel structures of potential use in shortwave magneto-optical22 and spintronic devices.23 In addition, semiconductors doped with small quantities of transition metals (TM), known as diluted magnetic semiconductors (DMS), are of great technological interest given their capacity to control spin as well as electric charge, a property that makes them potentially useful in the manufacture of new generation spintronic products.24
In addition, ZnO and TM doped ZnO compounds (such as Cr, Mn, V) exhibit photocatalytic applications under UV and solar radiation.25,26 ZnO:Mn also processes the capacity to capture CO2 and SO2.27 All of this makes these compounds potentially useful in several technological applications.
A number of studies have reported various ways of synthesizing the spinel ZnMn2O4. Courtel et al. synthesized ZnMn2O4 nanoparticles from their corresponding acetates via a hydrothermal process28 and via coprecipitation.29 The production of ZnMn2O4 microspheres via solvothermal synthesis from the corresponding acetates has been also reported.30 Recent studies have also shown that ZnMn2O4 spinel can be obtained via autocombustion processes31,32 and sol–gel methods,33,34 among others. However, while several authors have described the recovery of different valuable metals from spent lithium ion batteries,35–38 few of them describe in detail a comparative study of the structural characteristics and magnetic properties of these type of compounds.
The present work describes the synthesis of ZnxMn3−xO4 (0.25 ≤ x ≥ 1.25) compounds with molar ratios ranging between 1.4 and 11, and with a spinel crystalline structure, via coprecipitation from the solution obtained following the acidic leaching of spent battery black mass.35–38
Compound | Black mass |
---|---|
Na2O | 7.75 |
MgO | 0.23 |
Al2O3 | 0.46 |
SiO2 | 1.69 |
P2O5 | 0.99 |
SO3 | 0.64 |
Cl | 1.76 |
K2O | 6.70 |
CaO | 0.36 |
TiO2 | 0.191 |
MnO | 43.30 |
Fe2O3 | 1.42 |
Co3O4 | 0.03 |
NiO | 0.28 |
CuO | 0.08 |
ZnO | 26.88 |
SrO | 0.04 |
ZrO2 | 0.01 |
Nb2O5 | 0.01 |
CdO | 0.01 |
SnO2 | 0.03 |
BaO | 0.13 |
La2O3 | 0.05 |
CeO2 | 0.10 |
PbO | 0.04 |
Ctotal | 8.20 |
S | 0.24 |
Fourier-transformed infrared spectroscopy (FTIR) using a Varian 670 FTIR spectrometer (spectral range 1600–400 cm−1, spectral resolution of 4 cm−1) in transmittance mode was also performed. In addition, micro-Raman spectra were obtained using a confocal Horiba Jovin-Yvon LabRAM HR800 system. The samples were excited by a 633 nm He–Ne laser on an Olympus BX 41 confocal microscope with a 10× objective.
The temperature dependence of the magnetic susceptibility was measured in the 2–300 K range in a magnetic field of 1000 Oe using a Quantum Design XL-SQUID magnetometer. Hysteresis measurements were taken at 10 K with a maximum field of 5 T.
The surface chemistry of the BMO samples was examined by XPS. Spectra were recorded using a Fisons MT500 spectrometer equipped with a hemispherical electron analyzer (CLAM2) and a non-monochromatic Mg Kα X-Ray source operated at 300 W. Spectra were collected at a pass energy of 20 eV (typical for high-resolution conditions). The area under each peak was calculated after subtraction of the S-shaped background and fitting the experimental curve to a combination of Lorentzian and Gaussian lines of variable proportions. Binding energies were calibrated to the C 1s peak at 285.0 eV. The atomic ratios were computed from the peak intensity ratios and reported atomic sensitivity factors.40
ZnO (s) + 2H+ → Zn2+ (aq) + H2O (aq) | (1) |
ZnMn2O4 (s) + 6H+ + H2O2 → Zn2+ (aq) + 2Mn2+ (aq) + 4H2O (aq) + O2 (g) | (2) |
Sample (acid leaching) | Element | Lixiviation yield (%) | ||
---|---|---|---|---|
Zn | Mn | Zn | Mn | |
L1 | 24.8 | 88.8 | 81.0 | 99.8 |
L2 | 35.9 | 116.9 | 77.9 | 88.9 |
L3 | 48.6 | 101.6 | 79.4 | 60.0 |
L4 | 63.0 | 63.2 | 73.0 | 47.0 |
Table 2 reveals how the Mn content decreases as the amount of dissolved black mass increases. The highest Mn content was obtained for Li200 sample. The concentration of Zn increases with the amount of black mass dissolved.
During the alkaline precipitation process, the precipitation of Zn(OH)2 (eqn (3)) starts at pH 7.5 and increases with the pH. The precipitate was white.
Zn2+ (aq) + OH− (aq) → Zn(OH)2 (s) | (3) |
Zn(OH)2 (Ksp at 25 °C = 3 × 10−16) continues to form until a pH of 11.5 is reached, after which (bearing in mind the amphoteric nature of this compound) it dissolves to form zincate ions (eqn (4)):
Zn(OH)2 (s) + OH− (l) → ZnO22− (aq) + 2H2O (aq) | (4) |
The Mn2+ is stable up to pH 8.5, after which manganese hydroxide (Kps = 2.5 × 10−13) is formed, along with mixed Zn/Mn hydrates (eqn (5)):
xZnO22− (aq) + (3−x)Mn2+ (aq) + 2xOH− (aq) → ZnxMn3−x(OH)2x (s) | (5) |
These hydrated oxides are rapidly oxidized to form anhydrous oxides with a spinel structure (eqn (6)):
ZnxMn3−x(OH)2x (s) + 2O2 (g) → ZnxMn3−xO4 (s) + 2xH2O (aq) | (6) |
Depending on the Zn and Mn contents of each solution, the obtained value of x is different, ranging from 0.25 to 1.2. When x = 1, the product is ZnMn2O4 (sample BMO3). XRF analysis of BMO3 reveals a Zn content of 21.6 wt% and a Mn content of 49.6 wt%, similar to the stoichiometric values obtained (27.3 wt% Zn and 45.9 wt% Mn).
Ameri et al.41 proposed a similar mechanism for the formation of ZnMn2O4 via the electrodeposition of Zn2+ and Mn2+ solutions obtained from the dissolution of zinc and manganese nitrates. In their work, the initial solutions possessed an excess of Mn2+ in relation to the stoichiometry of ZnMn2O4 and therefore they obtained nanostructured ZnMn2O4/Mn3O4. Song et al.42 proposed a similar mechanism for the formation of ZnMn2O4 via solvothermal synthesis dissolving zinc and manganese nitrates solutions in citric acid and cetyltrimethyl ammonium bromide (CTAB).
The reactions shown above explain the formation of the Zn/Mn BMOs. In the case of BMO4 large amounts of ZnO were detected. This is a consequence of the high concentration of Zn2+ in the acidic solution (63.0 g L−1); during the alkaline precipitation process some Zn2+ did not combine with the Mn2+. This excess Zn2+ precipitated out as Zn(OH)2, and later became ZnO through dehydration.
Regarding the composition, with the exception of the odd minority elements, all are composed of Zn and Mn, the exact content of each depends on the amount of solution subjected to alkaline precipitation The Zn and Mn contents and stoichiometry as determined by XRF (Table 3) and Rietveld refined XRD (Table 4) respectively agrees quite well for samples BMO1, BMO2 and BMO3. The contents Zn and Mn for BMO1 (22.8 wt% and 49.2 wt%) agrees with the stoichiometric proportion for the Zn0.85Mn2.1504 phase (23.4 wt% and 49.7 wt% respectively). In the case of BMO2, the Zn and Mn contents are 8.1 wt% and 66.2 wt% respectively, which agrees with the stoichiometric proportion for the Zn0.25Mn2.75O4 phase (7.1 wt% and 65.3 wt% respectively). In the case of BMO3, the agreement is also good, the Zn and Mn contents of BMO3 are 26.7 wt% and 46.3 wt% respectively, while the stoichiometry of the ZnMn2O4 phase is 27.3 wt% Zn and 45.9 wt% Mn. However, a discrepancy seems to appear for the Zn and Mn contents of BMO4, since according to stoichiometry (Zn1.25Mn1.75O4) the expected values for the contents of both elements are 29.5 wt% and 36.5 wt% respectively, while from the XRF data, the Zn content is 40.2 wt% (Table 3). Nevertheless, if we take into account the data from Table 4, in this sample, an equivalent amount of ZnO (12% wt) is detected, then accounting for the 10.7 wt% excess of Zn observed.
Sample | Content (wt%) | Extraction efficiency (%) | ||
---|---|---|---|---|
Zn | Mn | Zn | Mn | |
BMO1 | 22.8 | 49.2 | 19.2 | 64.3 |
BMO2 | 8.1 | 66.2 | 16.8 | 86.2 |
BMO3 | 26.7 | 46.3 | 46.7 | 72.0 |
BMO4 | 40.2 | 36.0 | 82.3 | 48.0 |
Sample | Mineralogical composition (%) | Cell parameters of samples | |
---|---|---|---|
a (Å) | c (Å) | ||
BMO1 | Zn0.85Mn2.2104 (95%) | 5.756 | 9.266 |
Impurities (5%) | — | — | |
BMO2 | Zn0.25Mn2.7504 (95%) | 5.766 | 9.393 |
Impurities (5%) | — | — | |
BMO3 | ZnMn204 (96%) | 5.758 | 9.240 |
— | — | ||
BMO4 | Zn1.25Mn1.7504 (72%) | ||
ZnO (12%) | 5.789 | 8.976 | |
Impurities (16%) | — | — |
Table 4 shows the composition of the crystalline phases of the BMOs as determined by Rietveld refinement; where a very clear variation in the proportions of Zn and Mn is observed. The different Zn/Mn BMOs obtained also show a very high purity (95–96%).
The measured value for the a lattice parameter of the ZnMn2O4 phase is 5.758 Å, i.e., slightly higher than the values reported in the literature (5.709–5.722 Å). The value for b parameter (9.240 Å), however, is much closer to previously reported values (9.222–9.238 Å).37,41,42 The value of a parameter for the Zn/Mn BMO stoichiometries decreases with increasing Zn content. This agrees with previous results reported for ZnMn2O4 phases obtained by the ceramic method.43
The intensities of the diffraction maxima decrease as the Mn content increases. An increasing Mn content is therefore associated with a reduction in the crystallinity of the BMOs. Other authors have reported similar results for ZnO doped with Mn obtained via hydrothermal and sol–gel synthesis.44,45
Fig. 4 shows SEM images of the different BMOs. All reveal agglomerated particles of near-spherical morphology, similar to those reported for other samples of similar composition.46 No changes in this morphology are observed with the variation in the Zn/Mn content. Tetragonal crystals characteristic of the spinel phase are also visible (parts a and b of this figure).
Fig. 4 SEM images of the binary metallic oxides synthesized: (a) BMO1; (b) BMO2; (c) BMO3 and (d) BMO4. |
Fig. 5 shows TEM images of the different BMOs. Two different morphologies are present. In BMO1, BMO2 and BMO3 samples, spherical particles are mainly observed, while in BMO4 both spherical and hexagonal-shaped particles are visible. The hexagonal shaped particles could be related to the higher content of ZnO particles21 in agreement with our results of the Rietveld analysis (see Table 3). The mean diameter of the particles is 40, 50 and 35 nm for BMO1, BMO2 and BMO3 respectively. An increase in the Mn content leads to an increase in particle size, as previously reported.43
Fig. 6 shows the FTIR spectra for the BMOs. All show two main absorption bands at approximately 527 and 634 cm−1. These may be respectively attributed to distortion vibration of Mn3+ cations in an octahedral environment, and stretching vibration at Mn–O tetrahedral sites. A weaker band is also observed at around 420 cm−1, due to stretching vibration of Mn3+ at octahedral sites.44–46
Fig. 7a shows the normalized Raman spectra for the different ZnxMn3−xO4 samples. In all the spectra the bands are attributable to ZnMn2O4. These results are consistent with those obtained in the XRD analysis.
Fig. 7 (a) Normalized Raman spectra for different Zn/Mn ratios, and (b) zoom of the Raman peak in the 645–670 cm−1 range. |
According to the group theory, oxides of the stoichiometry XMn2O4 (where X = Zn, Mn) with a spinel-type crystalline structure and I41/amd space group have 10 active Raman modes: Γ = 2A1g + 3B1g + B2g + 4Eg.47 However, the present spectra do not show all these modes; indeed, the maximum number ever observed has been seven.48,49 The vibration modes above 600 cm−1, correspond to the movement of oxygen atoms in the tetrahedral AO4 groups, and reflect an A1g symmetry.
The low frequency modes are characteristic of octahedral sites (BO6). Other authors report a high variation in the position of the Raman peaks for ZnMn2O4. Malavasi et al.48 reported peaks at 300.2, 320.5, 381.9, 475.5 and 677.6 cm−1, Tortosa et al.49 at 276, 316, 320, 369, 463, 563, 630 and 663 cm−1, and Li et al.50 at 171, 321, 384, 476, 635 and 677 cm−1. In the present work, these peaks appear around 301, 350, 477 and 648 cm−1. The band in the 645–670 cm−1 range might be attributed to manganese oxides and Zn/Mn complexes.47 Fig. 7b shows a zoom of this Raman peak. Note that as the Mn content increases, the height of the peak decreases. According to XPS, in the sample with the higher Mn content, the predominant oxidation state is Mn2+, hence the differences observed in the Raman peak could be explained by the substitution of Zn2+ by Mn2+ (which is larger) in the BMOs,51 which would lead to a reduction in the bond distances. In addition, a broadening of the Raman bands can be appreciated related to the purity and crystallinity of the samples. These results are in good agreement with those obtained from the Rietveld refinement where highest percentage of impurities leading to a broader Raman bands.
Sample | TN (K) | Ms (emu g−1) | Hc (Oe) |
---|---|---|---|
BMO1 | 24.1 | 6.17 | 1720 |
BMO2 | 25.5 | 13.19 | 1720 |
BMO3 | 19.7 | 5.86 | 1220 |
BMO4 | 15.5 | 1.56 | 940 |
Different theories exist regarding the magnetic properties of (Zn, TM) O-type (with transition metals) oxides. Sharma et al.53 and Kundaliya et al.54 explain the ferromagnetism of these materials by assuming a uniform distribution of Mn in a ZnO matrix, or through the existence of phases with a ZnxMn2−xO3 stoichiometry stabilized by oxygen vacancies. Others explain it via the coexistence of Mn atoms in different states of oxidation.55 Fig. 9 shows the XPS spectra for the 2p Mn structure of each BMO. The bond energies for Mn 2p3/2 of MnO, Mn2O3 and MnO2 fall within the ranges 640.6–641.7, 641.7–641.9 and 641.9–642.6 eV respectively.56,57 Table 6 shows the elemental atomic percentages for the different Zn/Mn ratios, and the percentages according to the Mn oxidation state. In all the examined BMOs, mixtures of Mn2+, Mn3+ and Mn4+ are obtained. The XPS spectra for the O 1s are also shown in Fig. 9. In all cases, the obtained spectra exhibit asymmetric peaks. In this respect, there is a controversy in the interpretation of O 1s XPS spectra for different oxides. The band peaked at around 534 eV in some cases is attributable to hydroxyl groups OH, or other radicals on the sample surface58,59 or oxygen vacancies.60,61 For the present BMOs, none of these possibilities can be ruled out. Either, the existence of oxygen vacancies created to compensate the electric charge or the different Mn ions could be equally responsible for the magnetic behavior.
Sample | Atomic ratio Mn/Zn | Mn2+ | Mn3+ | Mn4+ |
---|---|---|---|---|
BMO1 | 8.3 | 14.5 | 3 | 7.8 |
BMO2 | 12.2 | 15.4 | 4.4 | 8.5 |
BMO3 | 1.3 | 6.3 | 7.3 | 5.5 |
BMO4 | 0.6 | 3.4 | 2.1 | 7.1 |
Fig. 10 shows the magnetization curves versus applied field. All are representative of a ferromagnetic material with magnetic domains. As expected, the magnetic saturation (Ms) increased with the Mn content, reaching a value of 13.2 emu g−1 for BMO2. Table 5 shows the different Ms values obtained for the BMOs in a coercive field (Hc). Ms decreases with increasing Zn content, a consequence of the presence of its non-magnetic cations.52 This was particularly clear for BMO4, which has the lowest Zn/Mn ratio and Mn mainly in the Mn4+ oxidation state (as determined by XPS). Thus – in agreement with other authors who have studied spinel BMOs of ZnxMn3−xO4 stoichiometry52 – the magnetic properties of the present BMOs can be explained according to a model of nanometric-scale ferrimagnetic clusters of Mn3O4 in an antiferromagnetic ZnMn2O4 matrix.62,63 These results are in good agreement with previous studies on ZnxMn3−xO4 phases formed by members of Mn3O4 and ZnMn2O4. The Mn3O4 phase contains Mn in oxidation state II at tetrahedral positions, and in state III at octahedral positions. As the Zn content increases (with increasing x in the stoichiometry ZnxMn3−xO4), the tetrahedral sublattice occupied by Mn2+ begins to be occupied by Zn2+. Table 6 shows how, in most cases, an increase in x is accompanied by a reduction in Mn2+ and an increase in Mn3+. The existence of Mn4+ can be explained by the presence, in some samples, of MnO2-type impurities (detected during Rietveld refinement analysis) or oxygen vacancies, as suggested by Kundaliya et al.54