Jianghao Wangab,
Liping Lic,
Lingshen Mengc,
Liping Wangc,
Yifeng Liuc,
Wenwen Lic,
Wengang Sunc and
Guangshe Li*ac
aKey Laboratory of Design and Assembly of Functional Nanostructures, Fujian Institute of Research on the Structure of Matter, Chinese Academy of Sciences, Fuzhou 350002, P. R. China. E-mail: guangshe@jlu.edu.cn
bUniversity of Chinese Academy of Sciences, Beijing 100049, P. R. China
cState Key Laboratory of Inorganic Synthesis & Preparative Chemistry, College of Chemistry, Jilin University, Changchun 130012, P. R. China
First published on 12th October 2018
The morphology of nano-arrays plays an important role in their applications for catalysis, energy, environment. However, the morphology modulation of nano-arrays generally involves complex optimization of synthetic conditions including surfactants, pH, and solvent. In this work, we synthesize a NiMoO4·H2O nano-array by a simple hydrothermal method under mild conditions (pH = 6.47, aqueous solution, and without the aid of surfactants). The morphology modulation of the NiMoO4·H2O nano-array is realized by simply changing the hydrothermal temperature. When the hydrothermal temperature below 150 °C, a NiMoO4·H2O nanorod array is obtained. While the hydrothermal temperature is as high as 180 °C, the array on Ni foam is nanosheet instead of nanorod. The NiMoO4·H2O nanorod array synthesized at 150 °C shows a superior water splitting activity compared to the NiMoO4·H2O nanosheet array, affording a large current density of 10 mA cm−2 at an overpotential of <240 and 200 mV toward oxygen evolution reaction and hydrogen evolution reaction, respectively. Furthermore, the electrolyzer using NiMoO4·H2O nanorod array as both anode and cathode electrodes for catalyzing overall water splitting exhibits great performance, obtaining a current density of 10 mA cm−2 at 1.67 V, comparable to the integration of commercial noble-metal Pt/C and IrO2 electrodes.
Nanoarrays grown on a substrate exhibit great potential for water splitting due to the following advantages: (i) nanoarray can be directly used as a working electrode for water splitting without the aid of polymer binders, which is beneficial for exposing active sites promoting electrolyte penetration; (ii) nanoarray has a strong interaction with the conductive substrate, which facilitates electron transportation;9,10 (iii) nanoarray structure is propitious to the superaerophilic ability of electrode, and thus release H2 or O2 easier during water splitting.11–13 Fascinated by the merits of nanoarray, various nanoarrays, such as nanorod, nanosheet, and hierarchical structure have been synthesized successfully by precise chemical methods. But, it is still hard to realize the morphology change of nanoarray selectively by a simple optimization. The syntheses of these nanoarrays generally involve complicate optimizations of reaction conditions including surfactant, pH, and dissolvent, which damage their further application.14–17 Therefore, it is an emergency to develop a new simple method to modulate the morphology of nanoarray.
To this end, we take NiMoO4·H2O as an example, the modulation of nanoarray morphology from nanorod to nanosheet is realized by simply changing the hydrothermal temperature without the aids of surfactants or additives. We can obtain nanorod array when hydrothermal temperature below or equal to 150 °C. While the hydrothermal temperature is as high as 180 °C, the array on Ni foam is nanosheet instead of nanorod. In addition, the performance of NiMoO4·H2O nanorod array as bifunctional catalysts toward overall water splitting depends highly on the hydrothermal temperature in the sample preparation. When hydrothermal temperature equals to 150 °C, the obtained sample shows a superior OER and HER activity performance separately, affording a large current density of 10 mA cm−2 at an overpotential of <240 and 200 mV toward oxygen evolution reaction and hydrogen evolution reaction, respectively. As expected, the electrolyzer using NiMoO4·H2O nanorod array as both anode and cathode for catalyzing overall water splitting exhibited the great performance, obtaining a current density of 10 mA cm−2 at 1.67 V, comparable to the integration of commercial noble-metal Pt/C and IrO2 electrodes.
To investigate the growth mechanisms of nickel molybdate hydrate nanoarray, we did some control experiments including the Ni-salt precursor, hydrothermal time, conductivity substrate, and concentration of Ni-salt precursor. Detailed experimental conditions are shown in Table S1.†
For the comparative purpose, the different control materials in powdered forms (Pt/C, IrO2) were drop-casted on Ni foam. Their amount and working surface area were kept the same as those used for NMO-150. In typical procedure: (1) 7 mg of catalyst was dispersed in 1 mL mixture of 450 μL de-ionized water, 500 μL ethanol and 50 μL 5% Nafion to form a homogeneous mixture, (2) 500 μL of this solution was drop-casted onto Ni foam electrode with an area of 1 cm2 and a loading amount of 3.5 mg cm−2, and left to dry in air.
Fig. 1 (A) Schematic illustration of the preparation process for NiMoO4 hydrate array and (B) photography of the bare Ni foam (left) and NMO-150 (right). |
To optimize the synthetic temperature of the growth of nanoarray, we adjusted the reaction temperature from 120 °C to 180 °C. The phase structures of NiMoO4·H2O nanoarrays were characterized by X-ray diffraction (XRD, Fig. 2). As shown in Fig. 2, the nanoarrays prepared under 120, 150, and 180 °C have a similar XRD pattern. In addition, the diffraction peak of XRD pattern in Fig. 2 agrees well with the data for NiMoO4·H2O (JCPDS no. 13-0128), revealing that all nanoarrays grown on Ni substrate are NiMoO4·H2O.18 In addition, Raman spectroscopy is used to monitor the structure of NMO-150. As shown in Fig. S1,† a set of Raman peaks are observed at 805, 831, and 938 cm−1, which are in consistent with previously reported Mo–O vibrations of NiMoO4.19 The Raman spectrum also demonstrates the existence of NiMoO4·H2O in the sample.
Fig. 2 XRD patterns for NMO-120, NMO-150, NMO-180. The data were recorded for the powder that was scraped from Ni foam. |
Fig. 3 shows the scanning electron microscopy (SEM) images of NMO-120, NMO-150, and NMO-180. The low-magnification SEM images in the left panel (Fig. 3(A, C, and E)) reveal that all samples are covered by a rough shell, indicating the successful growth of NiMoO4·H2O nanoarrays. The high-magnification SEM images shown in Fig. 2(B and D) demonstrate that the nanorods are covered on Ni foam for the samples that were obtained at the hydrothermal temperature of 120 °C or 150 °C. Comparatively, when the hydrothermal temperature is as high as 180 °C, the array on Ni foam is nanosheet instead of nanorod (Fig. 2F). This interesting finding demonstrates that hydrothermal temperature is an important parameter for the growth of nanoarrays. Different morphology of nanoarray from nanorod to nanosheet can be obtained by simply changing the hydrothermal temperature without the aid of surfactants or additives. The effect of temperature on the growth of nanoarrays is changing the Ni source that reacts with MoO42− ions from Ni2+ ions to Ni foam. When the reaction temperature below or equal to 150 °C, MoO42− ions react with Ni2+ ions in the solution, and then NiMoO4·H2O nanorods grow on the Ni foam directly. While reaction temperature equal to 180 °C, MoO42− ions react with Ni foam directly to form nanosheet array,20,21 which impedes the growth of NiMoO4·H2O nanorod. To verify this suppose, some control experiments were performed (Table S1†). Firstly, we changed the Ni-precursor by NiCl2·6H2O and NiSO4·6H2O. From Fig. S2,† we find that nanorod array can still be obtained under similar reaction conditions when using NiCl2·6H2O and NiSO4·6H2O as Ni-salt precursor, which demonstrate that the change in Ni-precursor has little effect on the morphological evolution. Secondly, we have replaced Ni foam with carbon cloth under the 180 °C for 6 h. As shown in Fig. S3,† we find that nanorod instead of nanosheet array can be obtained, providing the evidence of that the Ni2+ ions of NMO-180 are origin from Ni foam. Thirdly, we have changed the concentrations of Ni-salt (0, 6 mmol) to investigate the contribution of Ni2+ ions. From Fig. S4,† one can find that when the concentration of Ni-salt was 0 mmol, only the nanosheet array can be obtained, indicating that when Ni2+ ions come from the Ni foam, the dimensional anisotropy would be changed from 1D to 2D. When the concentration of Ni-salt was 6 mmol, only the nanorod array can be obtained, suggesting that additional contribution of Ni2+ ions would not result in the sheet-like structure.
NMO-120, NMO-150, NMO-180 were prepared under different hydrothermal temperature, which might result in a different activity for water splitting. To verify this suppose, the catalytic tests of oxygen evolution reaction (OER) and hydrogen evolution reaction (HER) for these three samples were performed in 1 M KOH electrolyte (Fig. S5 and S6†). As shown in (Fig. S5 and S6†), the sample of NMO-150 exhibits superior catalytic performance both in the OER and HER processes than other samples. This is because of the following two reasons. On the one side, the thickness of NiMoO4 films over Ni foam varied with hydrothermal temperature. From Fig. S5,† we can find that the oxidation peak of Ni2+/Ni3+ become weak with the increase of hydrothermal temperature, suggesting that the thickness of NiMoO4 films also become thinner. The nanosheet grown on the Ni foam would impede the growth of NiMoO4·H2O nanorod and decrease the amount of active species on the Ni substrate. Therefore, NMO-180 may have a less activity than NMO-150. On the other side, although nanorods covered Ni foam were prepared at both 120 °C and 150 °C, higher temperature (150 °C) could enhance the synergistic effect between NiMoO4 and Ni foam, which is beneficial to catalysis. Hence, the reaction temperature of 150 °C is the optimum condition for the growth of NiMoO4·H2O nanorod array, and thus NMO-150 is picked to systemically study its physical properties and catalytic performances.
To study the effect of hydrothermal time on the growth of nanorod array, we controlled the hydrothermal time (2 h, 4 h) under similar condition. From Fig. S7,† we can find that the samples treated by the hydrothermal method for 2 h and 4 h have a rod-like structure. With the increase of hydrothermal time, the length of nanorod become longer, which demonstrate that the growth mechanism of nickel molybdate hydrate nanoarray obeys the orientation attachment growth. Transmission electronic microscope (TEM) was performed to further reveal the morphology of NMO-150. As shown in Fig. 4A, the nanorod with a size about 150 nm in diameter can be clearly seen, which is consistent with the observation of SEM. Moreover, a large number of mesopores can be found easily on the surface of the nanorod. Measurements of isothermal (77 K) N2 adsorption and desorption for NMO-150 were performed to characterize the surface area and porosity of the product (Fig. S8†). The average pore diameter of the NMO-150 is about 3–5 nm to the desorption data (Fig. S8†). The existence of the mesoporous structure can not only increase the surface area of the catalyst but also provide more defects to produce an excellent catalytic performance. The corresponding high-resolution TEM (Fig. 4B) shows that the spacing between two adjacent lattice fringes is 4.03 Å.
The detailed surface chemical feature of NMO-150 was further determined by X-ray photoelectron spectroscopy (XPS). The XPS survey spectrum (Fig. 5A) shows typical signals of Ni, Mo, O elements, consistent with EDS analysis (Fig. S9†). In the Mo 3d core-level spectrum (Fig. 5A), two peaks at 232.2 and 235.3 eV are attributed to Mo 3d5/2 and Mo 3d3/2 respectively, and the spin-orbital splitting is about 3.0 eV (ΔMo 3d). The values for the binding energy of Mo 3d5/2 and ΔMo 3d are the typical features of the Mo6+ ion,22 which suggests that valence state of Mo ions in NMO-150 is +6. The Ni 3p in Fig. 5C exhibits a complicate spectrum comparing to pure Ni2+ and metal nickel.21 In addition to the strong photoelectron peaks at 856.3 and 874.2 eV and two satellite peaks at high binding energy side, two peaks at low binding energy are also distinguished. Therefore, the Ni 2p spectrum was de-convoluted into two spin–orbit doublets. The strong doublet at binding energies of 856.3 and 874.2 eV is ascribed to Ni2+, while the other one at 852.3 and 869.3 eV is assigned to Ni0 that comes from Ni foam.23 The O 1s signals with binding energies of 530.7 eV and 532.7 eV correspond to oxygen species in lattice and hydrate, respectively.3,24 According to the above XPS results, it can be concluded that the valences of Ni, Mo, and O elements are +2, +6, and −2, respectively. These observations indicate that NiMoO4 hydrate nanorod array has been synthesized successfully through a convenient hydrothermal method.
Fig. 5 X-ray photoelectron spectrum of NiMoO4·H2O: (A) survey spectrum, (B) Mo 3d, (C) Ni 2p and (D) O 1s. |
We evaluated the electrocatalytic activity of NMO-150 for OER and HER in 1 M KOH solution by a typical three-electrode system, in which NMO-150 was tailored into 1 × 1 cm2 and directly used as the working electrode. For comparison, we also measured the electrocatalytic activity of Ni foam, Ni foam-supported of commercial IrO2. As shown in Fig. 6A, NMO-150 shows a remarkable catalytic activity toward OER, with a current density of ≈280 mA cm−2 at a small overpotential of 370 mV, which is superior to many electrocatalysts reported previously.20,25–28 Moreover, the activity of NMO-150 is apparently better than that of IrO2, the benchmark for OER. Specifically, NMO-150 achieves a current density of 100, 150, 200 mA cm−2 with small overpotentials of about 310, 330, 350 mV, respectively. Where to reach the current density of 100 and 150 mA cm−2, the IrO2 must be applied larger overpotentials of 340 and 370 mV, respectively. Furthermore, at an overpotential of 370 mV, the current density of NMO-150 is about two and six times larger than commercial IrO2 and Ni foam. These results confirm the excellent OER performance of NMO-150.
Fig. 6B shows a multi-step chronoamperometric curve of NMO-150 toward OER in 1 M KOH solution. The operated overpotential was applied starting at 1.23 V and ending at 1.73 V (vs. RHE) with an increment of 50 mV every 500 s. The current maintains stable at each potential in the whole range, from 50 to 550 mV, and the current also switch quite rapidly, suggesting that NMO-150 has an excellent stability in a wide current density range (0–400 mA cm−2) and good mass transport property.29
We also examined the catalytic property of NMO-150 toward HER in basic media. For comparison, the electrocatalytic activity of Ni foam and Ni foam-supported of commercial Pt/C (20 wt%) were measured under the same testing condition. As shown in Fig. 6C, although the activity of NMO-150 is lower than that of Pt/C (20 wt%), much higher than that of Ni foam. When overpotential is 0.3 V, the current density for NMO-150 is about 75 mA cm−2, which is nearly seven times larger than Ni foam. To evaluate the stability of NMO-150, current density–time (I–t) curves for OER and HER in 1 M KOH were recorded at the potential of 1.47 V and −0.25 V (vs. RHE). As shown in Fig. 6D, NMO-150 retains the current density at 15 mA cm−2 over as long as 10 h electrocatalytic OER and HER. This further demonstrates that NMO-150 is a highly stable electrocatalyst for both OER and HER in basic media.
The electrochemical double layer capacitances (EDLC) were measured to evaluate the active area of electrocatalysts. Fig. 7A compares the variation of current density with scan rate for NMO-150 and Ni foam. Their double-layer capacitance (Cdl) values can be calculated by the slopes.3,30,31 The value of Cdl for NMO-150 is 60.1 mF cm−2, about three times larger than Ni foam, indicating that NMO-150 possesses a larger active area among all samples studied. Electrochemical impedance spectroscopy (EIS) for NMO-150 and Ni foam was recorded in 1 M KOH solution at an overpotential of 270 mV to determine their electrical conductivity. The equivalent circuit is shown in Fig. S10.† As illustrated in Fig. 7B and Table 1, comparing to Ni foam, sample NMO-150 exhibits smaller Rct,2 (charge transfer resistance) and. The smaller Rct,2 suggests that the charge transfer in the NMO-150 is more fluent, which could give a higher reaction rate.32–34 Therefore, the excellent catalytic activity of NMO-150 can attribute to a large number of active sites and improved electrical conductivity.
Fig. 7 (A) Relationship between current density and scan rate, and (B) EIS Nyquist plots recorded at an overpotential of 270 mV for NMO-150 and Ni foam. |
Samples | Rs (Ω) | Rct,1 (Ω) | CPE1-p | Rct,2 (Ω) | CPE2-p |
---|---|---|---|---|---|
NMO-150 | 1.48 | 0.55 | 0.44 | 1.89 | 0.94 |
Ni foam | 1.36 | 0.19 | 0.77 | 3.03 | 0.72 |
Given our finding that NMO-150 has an exotic bi-functional property toward OER and HER, we assembled an electrolyzer with NMO-150 as anode and cathode to study its activity for overall water splitting (OWS). As illustrated in Fig. 8A, the electrolyzer using NMO-150 as anode and cathode affords current density of 10 mA−2 at 1.67 V (vs. RHE). Despite this current density value is slightly inferior to that of electrolyzer constructed by Pt/C–IrO2 couple, it outperforms state-of-the-art electrolyzers utilizing Co- or Ni-based bifunctional electrocatalysts for overall water splitting.34 Furthermore, the long-term stability of this system was also tested. When the static potential of 1.67 V was applied, the electrolyzer afforded a constant current density around 10 mA cm−2 and showed an excellent stability after testing for 10 h (Fig. 8B).
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c8ra07323f |
This journal is © The Royal Society of Chemistry 2018 |