Mehrdad
Asgari‡
a,
Sudi
Jawahery‡
ab,
Eric D.
Bloch
cd,
Matthew R.
Hudson
e,
Roxana
Flacau
f,
Bess
Vlaisavljevich
g,
Jeffrey R.
Long
bch,
Craig M.
Brown
ei and
Wendy L.
Queen
*a
aInstitute of Chemical Sciences and Engineering, École Polytechnique Fédérale de Lausanne (EPFL), CH-1051 Sion, Switzerland. E-mail: wendy.queen@epfl.ch; Tel: +41 216958243
bDepartment of Chemical and Biomolecular Engineering, University of California, Berkeley, California 94720, USA
cDepartment of Chemistry, University of California, Berkeley, California 94720, USA
dDepartment of Chemistry and Biochemistry, University of Delaware, Newark, Delaware 19716, USA
eNational Institute of Standards and Technology, Center for Neutron Research, Gaithersburg, Maryland 20899, USA
fCanadian Neutron Beam Centre, National Research Council, Chalk River Laboratories, Chalk River, Ontario K0J 1P0, Canada
gDepartment of Chemistry, University of South Dakota, Vermillion, South Dakota 57069, USA
hDivision of Materials Sciences, Lawrence Berkeley National Laboratory, Berkeley, California 94720, USA
iDepartment of Chemical Engineering, University of Delaware, Newark, Delaware 19716, USA
First published on 23rd April 2018
We present a comprehensive investigation of the CO2 adsorption properties of an isostructural series of metal–organic frameworks, M-BTT (M = Cr, Mn, Fe, Cu; BTT3− = 1,3,5-benzenetristetrazolate), which exhibit a high density of open metal sites capable of polarizing and binding guest molecules. Coupling gas adsorption measurements with in situ neutron and X-ray diffraction experiments provides molecular-level insight into the adsorption process and enables rationalization of the observed adsorption isotherms. In particular, structural data confirms that the high initial isosteric heats of CO2 adsorption for the series are directly correlated with the presence of open metal sites and further reveals the positions and orientations of as many as three additional adsorption sites. Density functional theory calculations that include van der Waals dispersion corrections quantitatively support the observed structural features associated with the primary and secondary CO2 binding sites, including CO2 positions and orientations, as well as the experimentally determined isosteric heats of CO2 adsorption.
Metal–organic frameworks are a broad class of solid adsorbents consisting of metal ions linked by organic ligands to form porous, crystalline arrays, and are being intensively investigated for various energy-relevant applications, including gas storage, gas separation, and catalysis. These materials possess significant advantages over other solid adsorbents, including unprecedented internal surface areas, impressive structural diversity, and facile chemical tunability. Given the numerous permutations of potential linker and metal combinations, a vast number of frameworks are accessible in principle; however, to identify and better tune the properties of any framework for a target application, such as CO2 capture, it is essential to first understand structure-derived function. One powerful approach is the study of isostructural families of frameworks differing only in the identity of the metal ion.7–9 For example, we have previously shown that a combined experimental and theoretical approach can afford important insights into the factors influencing CO2 adsorption in the M2(dobdc) (M = Mg, Mn, Fe, Co, Ni, Cu, Zn; dobdc4− = 2,5-dioxido-1,4 benzenedicarboxylate) series of frameworks.10 However, a lingering practical challenge to the conduction of such structure–property relationship studies is the need for reliable experimental adsorption and in situ diffraction data for a group of isostructural frameworks, which is often not available for many frameworks of interest.
One such family is the sodalite-type series M-BTT (M = Cr, Mn, Fe, Co, Ni, Cu, Cd; BTT3− = 1,3,5-benzenetristetrazolate),11–15 with a general formula of [(M4Cl)3(BTT)8]3−. The framework crystallizes in the cubic Pmm space group (no. 221) and features truncated, octahedral cages built up of six [M4Cl]7+ units and eight [BTT]3− ligands that are further interlinked to form an anionic, porous, three-dimensional network (Fig. 1). This material is somewhat unique among metal–organic frameworks in that it readily undergoes chemical substitution with a number of first row transition metals and has a high density of open metal sites that are accessible after heating the as-synthesized material under dynamic vacuum to remove coordinated solvent. These properties are exhibited by only a few other known framework families, namely M2(dobdc),16–25 M2(dobpdc) (M = Mg, Mn, Fe, Co, Ni, Zn; dobpdc4− = 4,4′-dioxidobiphenyl-3,3′-dicarboxylate),26 M2Cl2(bbta) (H2bbta = 1H,5H-benzo(1,2-d:4,5-d′) bistriazole) and M2Cl2(btdd) (H2btdd = bis(1H-1,2,3-triazolo[4,5-b],[4′,5′-i])dibenzo[1,4]dioxin),27 M2(m-dobdc) (M = Mg, Mn, Fe, Co, Ni; m-dobdc4− = 4,6-dioxido-1,3-benzenedicarboxylate),28 and M3(btc)2 (M = Cr, Cu, Zn, Mo, Ru; btc3− = 1,3,5-benzene tricarboxylate).29–32
The open metal sites of the M-BTT family have been shown previously to increase the surface packing density of hydrocarbon adsorbates,33 to exhibit strong and selective binding of framework guests,13,15,34,35 and also to provide a pathway to achieve charge transfer between frameworks and guest species,36 a desirable property for using metal–organic frameworks for the conversion of small molecules into value-added chemicals.37 Most relevant to this study, the open metal sites can improve CO2 uptake at low-pressures, which is a property of interest for flue gas separations in post-combustion capture technologies.6,38 The M-BTT family thus stands as an important system for experimental examination of the role of metal identity on CO2 adsorption and subsequent identification and validation of computational tools useful in varying chemical environments.
Herein, we present a comprehensive experimental and computational investigation of CO2 adsorption in M-BTT (M = Cr, Mn, Fe, Cu) analogs, using in situ powder neutron diffraction and periodic density functional theory (DFT) calculations in tandem. Powder neutron diffraction reveals for the first time a molecular level view of CO2 adsorption in M-BTT and facilitates rationalization of experimental CO2 adsorption isotherms. The experimentally obtained binding distances and enthalpies are further used to benchmark and evaluate the results of DFT calculations on M-BTT, as reported in this work and a previous study.35 Ultimately, it is expected that the insights gained will inform how existing and hypothetical frameworks can be most efficiently screened for CO2 adsorption applications.
It is important to mention that the M-BTT compounds in activated form can sometimes detonate upon exposure to air. As such, these materials should be handled with caution and in small quantities.
Additional high-resolution neutron diffraction data were collected on the C2 diffractometer at Chalk River Laboratories at the Canadian Neutron Beam Center using a 1.2 g sample of Cr-BTT. The sample preparation and data collection of the bare and CO2-loaded framework were carried out using procedures similar to those described above. A wavelength of 2.3704 Å was used to collect data from ∼2.8° to 117° in 2θ. For this experiment, the gas loading apparatus designed for the top-loading, closed cycle refrigerator was not equipped with line heaters, and, because of this, cold zones caused the CO2 to freeze in the gas line before complete adsorption could be achieved. As such, loadings higher than 0.5 CO2 per Cr metal were not achieved and data were recollected at NIST. However, we note that results from the refinements of the bare structure and low CO2 loading are similar to those obtained at NIST (see ESI, Tables S7, S8 and Fig. S22†).
Powder neutron diffraction data were analyzed using the Rietveld method, as implemented in EXPGUI/GSAS.40,41 The M-BTT models were based on those previously determined,12,13,15 with the scale-factor and unit cell allowed to vary. Fourier difference methods were employed to locate residual solvent, extra-framework cations, and the adsorbed CO2 molecules in the structures of the activated bare materials.
X-ray diffraction data were also collected on Fe-BTT on 17-BM-B at the Advanced Photon Source at Argonne National Laboratory. The unactivated sample was loaded into a 1.0 mm borosilicate capillary that was then placed in a custom designed gas cell. The capillary was mounted onto the goniometer head at 17-BM and centered in the beam. The sample was then placed under dynamic vacuum, inserted in a N2 stream that was slowly heated to 150 °C where it was held for 2 h. Post-activation, the sample was gradually cooled to room temperature and then dosed with a small amount of He exchange gas. The sample was then further cooled to 100 K at a rate of 2 K min−1 where it was held for 30 min prior to data measurement to allow for temperature equilibration. The data were collected using a Si (111) monochromator (λ = 0.61072 Å, ΔE/E = 1.5 × 10−4). It should be noted that while efforts to activate the sample in situ succeeded in removing some of the methanol from the framework channels, they were unsuccessful at removing any of the methanol coordinated to the metal sites. Rietveld analysis was carried out on the data to elucidate the positions of extra-framework cations. Due to the inability to completely desolvated the framework at the synchrotron, data collection on the CO2-adsorbed samples were not pursued.
To gain a quantitative estimation of binding strength, we calculated isosteric heats (Qst) of CO2 adsorption, which afford a measure of the average binding energy at constant coverage and can be determined by fitting the adsorption isotherms with a dual-site Langmuir–Freundlich equation (Fig. S3–S6†). The calculated zero-coverage isosteric heats (Table 1) range from 30.7 kJ mol−1 to 51.2 kJ mol−1 with the trend Fe > Mn > Cr > Cu. Consistent with previous studies of the M2(dobdc) (M = Mg, Mn, Fe, Co, Cu, Zn) frameworks, the observed isosteric heats cannot be rationalized based upon ionic radii alone.10,57 A computational study of the M2(dobdc) series by Yu et al. revealed that the electrostatic interactions are likely dictated by nuclear screening effects that cause variations in the effective charge experienced by the CO2 at the open metal site.57 Computational work conducted both in this study on M-BTT frameworks (M = Cr, Fe, Cu) and an earlier work by Poloni et al. supports the experimentally observed trend in binding energy (Fe > Cr > Cu).35
M2+ | Isotherm | DFT (rev-vdW-DF2 + U) | Diffraction data | ||||||
---|---|---|---|---|---|---|---|---|---|
SA (m2 g−1) | Q st (kJ mol−1) | −Hb (kJ mol−1) | M–O(CO2)b | N⋯Cc | O–C–Od | M–O(CO2)b | N⋯Cc | O–C–Od | |
a Experimentally-determined surface areas (SA), zero-coverage isosteric heats of adsorption (Qst), and select geometric parameters for surface bound CO2 are presented; computed enthalpies of adsorption (−Hb) and select geometric parameters are included for comparison. Values in parentheses indicate one standard deviation. b Distance from the metal center to the bound oxygen of CO2. c Distance between carbon of bound CO2 and the nearest tetrazole nitrogen. d Intramolecular angle of bound CO2. e Due to the challenge of removing all solvent molecules bound to the open Mn2+ sites, data collection using neutron powder diffraction and DFT calculations on Mn-BTT were not pursued. | |||||||||
Cr | 1820 | 36.7 | 36.6 | 2.625 | 2.914 | 176.7 | 2.66(4) | 3.04(2) | 176(2) |
Mne | 2050 | 45.6 | — | — | — | — | — | — | — |
Fe | 1700 | 51.2 | 51.7 | 2.301 | 3.019 | 174.4 | 2.36(3) | 3.00(3) | 180(4) |
Cu | 1700 | 30.7 | 29.4 | 2.567 | 3.041 | 177.1 | 2.60(3) | 3.01(1) | 177(1) |
Upon increasing the CO2 loading, a rapid drop is observed in the isosteric heat for Fe- and Mn-BTT, likely indicating that a portion of the primary adsorption sites are blocked by residual solvent molecules. Indeed, previous in situ structural studies of D2 adsorption in this series of frameworks revealed a significant number of metal sites are blocked by solvent molecules that cannot be removed using standard activation procedures.11,13 Rietveld refinement of the neutron diffraction data collected in this study on the bare Cr-BTT, Fe-BTT, and Cu-BTT frameworks post-activation revealed that ∼23%, ∼65%, and ∼17% of the open metal sites, respectively, are blocked by coordinated solvent. Therefore, the overall trend for the number of available open metal sites follows the order Cu ≈ Cr > Fe > Mn, consistent with what has been previously reported.11,13,15 The smaller number of available open metal sites in Mn-BTT causes the isosteric heat to drop faster than that of the Fe-analog (Fig. 2), while the larger number of available open metal sites in Cu-BTT and Cr-BTT can be used to rationalize their higher overall capacity for CO2 at 1 bar, despite their lower zero-coverage isosteric heat of CO2 adsorption (Table 1).
Fig. 2 (Left) Excess CO2 adsorption isotherms obtained at 298 K for various M-BTT analogs. (Right) Isosteric heats of adsorption, Qst, plotted as a function of CO2 loading. |
Following structure determination of the activated materials, the samples were dosed with ∼0.5 CO2 per framework M2+ and the analysis was repeated. For all analogs, the primary adsorption site consists of CO2 bound in an end-on configuration at the M2+ cation (Fig. 1), confirming the presence of strong electrostatic interactions indicated by the high initial isosteric heats of adsorption. The M2+–O(CO2) distances range from 2.36(3) Å for Fe-BTT to 2.60(3) Å for Cu-BTT. While Cr-BTT binds CO2 more strongly than Cu-BTT, the similar M2+–O(CO2) distances in both analogs can be rationalized based on the larger ionic radii of Cr compared to Cu.
Secondary van der Waals interactions between the CO2 carbon atoms and the nitrogen atoms on the nearest tetrazole ring in each framework (located at a C⋯N distance of ∼3 Å) lead to M–O–C(CO2) angles ranging from 106(1)° for Cu-BTT to 116(2)° for Fe-BTT. DFT angles are overestimated for this parameter at 127.5° for Cu-BTT and 134.0° for Fe-BTT, but the trend between the metals is consistent with the experiment. Fe-BTT has the strongest binding energy and the largest angle. The computed angle for Cr-BTT is 126.3°, so Cr and Cu have similar binding angles despite Cr having a stronger binding energy; however, in the case of Cu, the presence of an extra-framework cation in the main adsorption cage could also influence the CO2 orientation. The intramolecular CO2 angles show minimal deviation from the expected linear geometry. While these angles are in good agreement with DFT calculations (Table 1) and indicate that there is little electronic activation of the bound CO2 molecule, nothing can be said about the trend in the CO2 angles due to the error associated with the diffraction experiment. The binding enthalpies and geometries of CO2 in M-BTT (M = Cr, Fe, Cu) were also determined by periodic DFT calculations, and the results are presented in Tables 1 and 2. The theoretical site I CO2 binding energies (Table 1) are in excellent agreement with experimentally-determined zero-coverage isosteric heats of adsorption, importantly capturing the observed experimental trend. The theoretical M–O(CO2) distances for site I (Table 1) in the Cr- and Cu-BTT frameworks are also in near perfect agreement with the experiment (differing by < 0.04 Å) and within the range of the standard deviation (Fig. 4 and S20†). The theoretical site I M–O(CO2) distance in Fe-BTT is also in excellent agreement with experiment (differing by < 0.06 Å). When considering the margin of error associated with the diffraction experiment (≈0.03–0.04 Å), there is almost no difference between the computationally and experimentally determined metal–oxygen distances for CO2 binding in Cr-, Fe-, or Cu-BTT. We note that the calculated M–O(CO2) distances are also in much better agreement with experiment than those previously predicted for the M-BTT series,35 which show deviations up to ∼0.2 Å (the values reported previously use a different flavour of DFT and different positions for extra-framework cations). While the calculated trend in M–O(CO2) binding distances (Cr ≈ Cu > Fe) presented here corresponds with the one observed experimentally, the Cr–O(CO2) bond distance is slightly longer than the Cu–O(CO2) distance despite the stronger Cr–CO2 binding energy. This is likely due to the aforementioned difference in the ionic radii of Cu2+ and Cr2+. Note that previous work by Poloni et al. reported that this distance correlated with binding strength; however, their calculated Cu–O(CO2) distance was only 0.005 Å longer than Cr–O(CO2) and therefore is also in good agreement with experiment.
M2+ | DFT (rev-vdW-DF2 + U) | Diffraction data | |||
---|---|---|---|---|---|
−Hb (kJ mol−1) | O⋯Cla | O–C–Ob | O⋯Cla | O–C–Ob | |
a Theoretical and computed bond distances describe the distance between the oxygen atom in CO2 and the chlorine atom in the center of the cluster. b The intramolecular O–C–O angle of the CO2 molecule. | |||||
Cr | 26.6 | 3.303 | 179.1 | 3.17(3) | 179(6) |
Fe | 24.5 | 3.237 | 179.7 | 3.38(2) | 179(7) |
Cu | 26.8 | 3.300 | 179.4 | 3.27(2) | 179(8) |
Upon increasing the CO2 loading from 0.5 to 1.5 CO2 per M2+, three additional, weaker adsorption sites become populated (Fig. 1). In the case of Mn- and Fe-BTT, the significant drop in their isosteric heats of CO2 adsorption (Fig. 2. (right)) indicates that preference for site I persists to room temperature. In contrast, the relatively flat nature of the isosteric heats of adsorption for Cr- and Cu-BTT implies similar binding energies for the different binding sites at room temperature, an observation that is supported by the predicted binding enthalpies of sites I and II determined via DFT calculations (Tables 1 and 2). A comparison of the DFT-derived CO2 binding energies for sites I and II provides further valuable insight into the behavior of the framework adsorption isotherms. While the binding energy of CO2 at site I depends strongly on metal identity, the binding strength at site II appears to be nearly independent of the metal. Indeed, the DFT binding strengths of CO2 at site II (Table 2) vary by only 2 kJ mol−1 across the frameworks studied. Given that the M-BTT frameworks are isostructural, it is perhaps unsurprising that CO2 should adsorb with similar binding energies at secondary adsorption sites. The DFT results are further supported by the similar isosteric heat values extracted for the frameworks at higher surface coverage (Fig. 2).
The secondary CO2 adsorption site in Cu-BTT (Fig. 1) is rotationally disordered above the [Cu4Cl]7− cluster. The closest oxygen atom of carbon dioxide bound at this site is approximately 3.27 Å from the Cl− and 3.44 Å from the center of the tetrazolate ring, distances that are in agreement with what is expected based on the van der Waals radii of oxygen and chlorine. Interestingly, the extra-framework cations in Fe-BTT also reside just above the Cl− anion in the [M4Cl]7− cluster and partially block the secondary adsorption site in this structure. In addition to the blocking of a large number of primary adsorption sites due to solvent molecules, the positioning of this cation may also influence the significant drop observed in the Qst for Fe-BTT relative to Cr- and Cu-BTT. As was the case for CO2 bound at site I, the DFT calculated binding geometries for CO2 at site II match well with the experimentally-determined values (Table 2). The largest deviation was observed for Cr-BTT, for which the DFT calculations revealed a Cl⋯O(CO2) distance that is ∼0.1 Å longer than that observed experimentally. The experimentally and theoretically determined structures for Cu-BTT are overlaid in Fig. 4 (see also Fig. S20†).
At site III, CO2 is rotationally disordered between two carbon atoms of the BTT3− linker and located at a C⋯O distance of ∼3.27 Å from the framework wall. Although this site is twice as abundant as site II, the adsorption of CO2 at site III is expected to be weaker given its lower occupation observed via in situ neutron diffraction. It should be noted that while the CO2 molecules located at sites III and IV are somewhat disordered, the intermolecular CO2 distances for these two sites are shorter than those of the closest CO2-framework distances. It may be that the population of site II helps to stabilize the population of these two additional adsorption sites, an observation that is supported by a pronounced plateau in Qst at higher loadings (Fig. 2). It is also possible that CO2 molecules located at sites III and IV afford additional stabilization to CO2 molecules located at site II (Fig. 1), in a manner similar to that suggested in an earlier study on CH4 binding in the metal–organic framework Cu3(btc)2.60
Positional disorder in the CO2 molecules bound at sites III and IV precluded periodic DFT analysis, and therefore we turned to force fields to quantify any stabilizing influence of neighboring CO2 molecules on the adsorbed gas at these positions. For this analysis, we arranged the site III and IV CO2 molecules at their experimental unit cell positions around site II CO2 with the DFT-determined binding geometry. We found the strength of the interaction between site II and site III CO2 molecules to be −4.58, −3.13, and −3.26 kJ mol−1 for Cu-, Cr-, and Fe-BTT, respectively. Interactions between CO2 located at site II and site IV were found to be smaller, although of the same order of magnitude. Considering the magnitude of the CO2 binding enthalpies at site II (Table 2), it is expected that interactions with CO2 molecules at sites III and IV are unlikely to have a large impact on the site II binding enthalpy. However, the CO2 molecules at sites III and IV exhibit weaker interactions with the framework compared to that of site II and may be primarily stabilized by interactions with the closest site II molecule.
Because the strength of CO2 binding at site I is dependent on the identity of the framework metal and the binding strength at site II is not, the theoretical difference between the site I and site II binding energies follows the same trend across the M-BTT series as the site I binding energy (Fe > Cr > Cu). DFT calculations show that CO2 binds more strongly at site I than site II in Fe-, Cr-, and Cu-BTT by 27.2, ∼10, and 2.6 kJ mol−1, respectively. The higher binding strength at site I is supported by the higher experimentally observed site I occupancy at low CO2 loadings in diffraction experiments. We note that while an energy difference as small as ∼3 kJ mol−1 is enough to distinguish sites I and II and lead to sequential occupation of adsorption sites at 10 K, at room temperature there is enough thermal energy such that there is no strongly preferred adsorption site. A similar phenomenon has been observed for CH4 binding in Cu3(btc)2 using powder neutron diffraction, wherein thermodynamic preference for a given binding site at 150 K is lost at higher temperatures.60 Room-temperature CO2 adsorption isotherms for Cr-, Fe- and Cu-BTT plotted on semi-log and logarithmic axes are shown in Fig. S18 and S19.† On a semi-log scale, Cr- and Cu-BTT exhibit Langmuir-type CO2 adsorption behavior, while in Fe-BTT CO2 appears to bind most strongly at low pressures. This latter observation is supported by DFT calculations, which predict the largest difference in site I and II binding energies for Fe-BTT. The combined theoretical and experimental work presented here suggests that differences in binding energy of >20 kJ mol−1 may be needed to observe a truly sequential loading of different binding sites in room temperature adsorption isotherms.
In particular, the site I binding energies and trend in M–O(CO2) distances reported previously are in good agreement both with those in this work and with the experimental isosteric heats of adsorption. This supports the conclusion that the interaction with the M2+ cation dominates and this site is not particularly sensitive to the position of the framework cation. On the other hand, the site I binding geometries from this study more closely match the diffraction results. For example, the M–O(CO2) binding distances at the primary adsorption sites were on average 0.045 Å closer to the experimental values compared to those reported previously. Our distances are slightly shorter than experiment while those of Poloni et al. are slightly longer. This could be due to the fact that the rev-vdW-DF2 functional was reparameterized specifically to improve bond distances while maintaining good binding energies; however, functional dependence in this system has not been systematically examined. The previous study also observed that stronger CO2 binding correlated with deviations from the expected linear geometry of CO2 and shorter distances between the tetrazole nitrogen and the CO2 carbon. In the diffraction results presented here, neither of these trends is observed. Although our DFT calculations started from the experimental structure, we observe the same trend in CO2 bending as Poloni et al. Moreover, the distance between the tetrazole nitrogen and CO2 carbon shows no clear dependence on the binding energy and the trend between the metals is different in the experiment (Cr > Cu > Fe), our calculations (Cu > Fe > Cr), and those of Poloni et al. (Cu > Cr > Fe). However, both experiment and Poloni et al. report the shortest N–C distance for the strongest binding metal. Additionally, in our calculations for Fe-BTT sodium migrated closer to Cl than the experimentally observed Fe cation. It is possible that the location and identity of the extra framework Fe cations has an impact on the CO2 binding geometry.
The diffraction data presented in this work has created the opportunity for a future benchmarking study to determine the influence of different DFT functionals on the accurate prediction of CO2 adsorption properties in the M-BTT framework series. Relative differences between Cr- and Fe-BTT structures computed in this work compared to the previous study may have to do with the placement of sodium cations, the respective choices of functional, and the choices in the level-of-theory. Furthermore, the specific identity of the extra-framework cations may play an important role in counterbalancing intra-framework forces. For example, DFT studies exploring whether extra-framework cations with different ionic radii and partial charge could occupy different sites based on steric effects, which has been suggested in the literature,61 have not been performed.
The foregoing results also provide experimental evidence that the strength of adsorption at the open metal site in the M-BTT series can be rationalized based on metal identity, including the partial charge on the electropositive M2+ cations. This observation is confirmed by both prior computational work and the results of DFT calculations presented here.35 DFT calculations also suggest that the heat of adsorption at site II is not dependent on metal identity. Strong CO2 adsorbents, like Fe-BTT, display sequential adsorption behaviour, which could potentially be exploited for applications such as CO2 conversion. This study shows the need for combined experimental and computational studies capable of predicting framework properties, a process that might eventually allow the rapid identification of target materials for CO2 capture, as well as a host of other applications.
Footnotes |
† Electronic supplementary information (ESI) available: Adsorption isotherms and its crystallographic information, additional figures, Fourier difference maps, and results from DFT simulations. The refined structures by powder diffraction: CCDC 1582001–1582011. For ESI and crystallographic data in CIF or other electronic format see DOI: 10.1039/c8sc00971f |
‡ These authors have contributed equally to this study. |
This journal is © The Royal Society of Chemistry 2018 |