Diana M.
Bobrowska
a,
Halyna
Zubyk
a,
Elzbieta
Regulska
a,
Elkin
Romero
b,
Luis
Echegoyen
b and
Marta E.
Plonska-Brzezinska
*c
aInstitute of Chemistry, University of Bialystok, Ciolkowskiego 1K, 15-245 Bialystok, Poland
bUniversity of Texas at El Paso, 500 W University Ave., Chemistry and Computer Science Bldg. #2.0304, El Paso, TX 79968-8807, USA
cDepartment of Organic Chemistry, Faculty of Pharmacy with the Division of Laboratory Medicine, Medical University of Bialystok, Mickiewicza 2A, 15-222 Bialystok, Poland. E-mail: marta.plonska-brzezinska@umb.edu.pl; Tel: +48 85 748 5683
First published on 3rd July 2019
Many macromolecular systems, including carbon nanostructures (CNs), have been synthesized and investigated as acceptors in photovoltaic devices. Some CNs have shown interesting electrochemical, photophysical and electrocatalytic properties and have been used in energy and sustainability applications. This study focuses on the covalent functionalization of carbon nanoonion (CNO) surfaces with ferrocene moieties to obtain donor–acceptor systems involving CNOs as acceptors. The systems were synthesized and characterized by infrared, Raman, UV-vis and fluorescence spectroscopies, thermogravimetric analysis, scanning electron microscopy, nitrogen adsorption and electrochemical measurements. The HOMO–LUMO levels were calculated to evaluate the possibility of using these systems in photoactive devices. In this study, for the first time, the CNO-based derivatives were applied as acceptors in the active layer of photovoltaic devices. This study is the first to use large CNO-based derivatives as acceptors in organic photovoltaic devices, and a power conversion efficiency as high as 1.89% was achieved.
Since 1994, C60 and its derivatives have been among the most frequently used acceptors in heterojunction OPV cells.11–14 Upon electron reduction, C60 presents a low reorganization energy.15 This property is due to the spherical rigid carbon framework and the delocalized π-electron system that contribute to the stabilization of the incoming charge with minimal structural or solution polarization changes.16 The delocalization of electrons or holes within the spherical carbon framework (diameter = 7.5 Å) offers unique opportunities for the stabilization of charges.17 Therefore, C60 can lead to fast photoinduced charge-separated (CS) states. Many reports have described the application of larger nanostructures, such as carbon nanotubes (CNTs)18–21 and endohedral fullerenes, instead of fullerenes.22–24 A promising direction proposed to improve cell efficiency is the incorporation of nanostructures, such as CNTs, which may facilitate charge separation and transport to the electrodes.25
Multi-shelled fullerenes, also known as carbon nanoonions (CNOs), can also be used as the acceptor in photovoltaic systems. Because of their unique spherical structures, CNOs can readily be covalently and non-covalently integrated into macromolecular systems due to their sp2-hybridized carbons.26 CNOs prepared from nanodiamond particles (NDs, 5 nm diameter) via thermal annealing process consist of 6 to 8 layers and are 5–6 nm in diameter.27,28 These spherical CNs possess very interesting physico-chemical properties, including electronic ones. The spherical CNOs obtained from NDs are paramagnetic and have unpaired electrons on their surfaces.29 The conductance of thiol-functionalized CNOs (synthesized at 1650 °C) in a molecular junction were investigated using scanning tunnelling microscopy.30 The study demonstrated that the electron transmission through CNOs occurred by a tunnelling mechanism, and the values were comparable to those of metallic nanowires. These unusual properties of CNOs prompted us to use them in OPVs as acceptor moieties in the active layer.
Some attempts have already been made to apply CNOs in photoactive devices. Since then, to the best of our knowledge, no reports on the use of CNOs as acceptor in the active layer of OPVs have been demonstrated.31,32 Notably, these CNs were used as hole collection layers in zinc-phthalocyanine-based OPV solar cells. The photocurrent was observed to increase by a factor of 5.5 over that of solar devices without CNOs.31 The highest power conversion efficiency (PCE) was up to 6.9 × 10−2%.31 Analogously, a device based on a crystalline perovskite film with oxidized CNOs incorporated into the hole transporting layer together with poly(3,4-ethylenedioxythiophene):polystyrene sulphonate (PEDOT:PSS), resulted in a significant enhancement of the PCE from 11.07 to 15.26%.32 Additionally, larger CNO structures (30 nm in diameter) were used in dye-sensitized solar cells as a counter electrode, and the PCE was comparable to that obtained with the commonly used platinum one.33
In the present study, we report the synthesis and photo- and electrochemical behaviour of some CNO-based systems prepared using different strategies. Five derivatives containing CNOs and covalently linked ferrocene derivatives were obtained, and their compositions were determined by several experimental methods. For the first time, the potential of such systems as acceptors in active layers in OPV devices is reported.
The synthetic procedures used to prepare the carbon nanoonion-ferrocene (CNO-Fc) systems are shown in Scheme 1. These derivatives were synthesized using five different approaches. The details of the synthetic procedures are described in the Experimental section. Briefly, in the first approach, CNOs were functionalized with ferrocenecarboxylic acid (CNO 2) via an acylation reaction of the amino-CNO derivative (CNO 1) (Scheme 1a). CNOs with carboxamide groups were obtained using oxidized-CNOs (ox-CNOs), which were functionalized according to a procedure previously described.26,34 In the second approach, CNO 4 was prepared in two steps first involving the functionalization of pristine CNOs with 4-aminobenzylamine (CNO 3) and then a reaction with ferrocenecarboxylic acid, as shown in Scheme 1b. The preparation of CNO 5 was performed using the reaction of 1,2-dicyanobenzene with phenol without any solvent, followed by reaction with CNO 3 in toluene. The CNO 5 derivative was further reacted with ferrocenecarboxylic acid. CNO 7 was obtained by the Diels–Alder addition of maleimide to pristine CNOs. Ferrocenecarboxylic acid was subsequently added to CNO 7, to obtain CNO 8 (Scheme 1d). The combination of 1,1′-bis(diphenylphosphino)-ferrocene with CNO 9 (Scheme 1e) resulted in the formation of CNO 10. The reaction was performed in the presence of isopentyl nitrite as a catalyst.
Scheme 1 Syntheses of the CNO-Fc derivatives: (a) CNO 1 and CNO 2, (b) CNO 3 and CNO 4, (c) CNO 5 and CNO 6, (d) CNO 7 and CNO 8, and (e) CNO 9 and CNO 10. |
The Fourier-transform infrared (FT-IR) spectra of pristine and functionalized CNOs are shown in Fig. 1. The ferrocene compounds (ferrocenecarboxylic acid and 1,1′-bis(diphenylphosphino)-ferrocene) were used as controls for comparison (see spectra Fig. 1c and 1l, respectively). The band at 1545 cm−1 for CNOs (Fig. 1a) corresponds to the CC stretching vibration. Two bands appearing at approximately 3020 and 995 cm−1 arise from C–H and CH2 stretching vibrations, which indicate the presence of defects in the CNO structures.29 Additionally, the two bands appearing at 1741 and 1245 cm−1 are assigned to CO bonds, which likely form during the annealing of CNOs in air at 400 °C.35 The main peaks in the IR spectrum of ox-CNO appear at 1710 and 1280 cm−1 and belong to the stretching vibrations of the C–O bonds formed during the oxidation process of graphite-like layers in the CNO structure (Fig. 1b).29
The intensities of the peaks in the 1440–1540 cm−1 region, associated with the CC stretching vibrations of the rings, decrease upon oxidation of the CC bonds. Ferrocene derivatives exhibit peaks in the 820–1960 cm−1 region,36,37 and the pattern depends on the molecular structure of the complex. The intense peaks at 1470, 1580 and 1950 cm−1 are assigned to the CC and C–H stretching vibrations of the rings. The band appearing at 1158 cm−1 and the two peaks at 926 and 830 cm−1 are assigned to C–H in-plane bending and out-of-plane deformations, respectively. The appearances of a broad band at approximately 3100 cm−1 for the O–H stretching vibration and strong peaks at approximately 1680 and 1285 cm−1 arising from CO stretching vibrations indicate the presence of carboxylic acid groups on the carbon nanostructures (Fig. 1c). After the first stage of the reaction, the CNO derivatives (CNO 1, CNO 3, CNO 5, and CNO 7) contain NH and NH2 groups (reactions a, b, c, and d; Scheme 1). The presence of peaks in the range of 3390–3420 cm−1, which correspond to N–H stretching vibration, can be used to monitor the presence of NH and NH2 groups. For these compounds, other peaks characteristic of the pristine CNOs are also observed. In the case of Fc-CNO derivatives CNO 2, CNO 4, and CNO 6, the stretching vibrations of N–H groups are noted. The bands appearing in the range from 1020–1295 cm−1 arise from C–N stretching vibrations, and they are discerned for all products from CNO 1 to CNO 8. The vibrational bands observed at frequencies in the range from 1665–1800 cm−1 for CO bonds indicate the successful modification of CNOs by ferrocenecarboxylic acid groups.
The reaction with the 1,1′-bis(diphenylphosphino)-ferrocene derivative results in changes in the FT-IR spectrum (Fig. 1l). The bands appearing at approximately 3060 and 830 cm−1 and in the range from 1480 to 1660 cm−1 are assigned to C–H and CC stretching vibrations of benzene rings, and those at 1970 and 1895 cm−1 are also assigned as the CC stretching vibrations of the benzene rings. The bands near 1085 cm−1 arise from C–P stretching vibrations. The spectrum of CNO 9 is shown in Fig. 1m and contains bands at 2820 and 2920 (CH3 bending vibrations), 2095 and 1875 (CC stretching vibrations of alkenes), 1655 and 1405 (CC stretching vibrations of the benzene rings), 1270 (C–O stretching vibrations) and 975 (C–H out-of-plane deformation vibrations) cm−1. The characteristic peaks at approximately 3000 and 865 cm−1, and at 1560 and 1450 cm−1 observed for CNO 10 correspond to the stretching and bending of C–H and the stretching bonds of CC groups in benzene rings (Fig. 1n). Therefore, the peaks at 1720 and 1265 cm−1 represent the stretching of C–O groups, and the peaks at approximately 1080 cm−1 are assigned to C–P stretching vibrations.
The Raman spectra excited at 514.5 nm of pristine and functionalized CNOs are shown in Fig. 2, and the data are collected in Table 1. For CNOs, the strongest features are observed at 1337 (D line) and 1576 cm−1 (G line), and the shifts of these bands for functionalized CNOs are summarized in Table 1. To measure the change in the position and intensity of Raman peaks, the spectra were normalized to the intensity of the G band and fitted by four Lorentz-shape components.38 For all pristine and functionalized CNOs, the D and G lines are intense and broad, and the D band is stronger than the G band. The functionalization of the CNs affects the G and D bands' positions and intensities. Decreasing the number of aromatic rings in the structure leads to a reduction in the frequency and intensity of the D band (Table 1). An increase in the line width of the D band also suggests an increase in the disorder of the functionalized CNOs. The G band appears at 1576 cm−1 for CNOs (Fig. 2a) and shifts to higher frequencies for the functionalized CNOs (Fig. 2b–k; see also Table 1). These observations can be explained by a decrease in the size of the aromatic segments upon functionalization.39 The intensity ratios (ID/IG) for pristine CNOs and their derivatives were also calculated (Table 1).
Fig. 2 Raman spectra (recorded at λext = 514 nm) of (a) CNOs, (b) CNO 1, (c) CNO 2, (d) CNO 3, (e) CNO 4, (f) CNO 5, (g) CNO 6, (h) CNO 7, (i) CNO 8, (j) CNO 9, and (k) CNO 10. |
Sample | D (cm−1) | G (cm−1) | 2D (cm−1) | I D/IG |
---|---|---|---|---|
CNO | 1337 | 1576 | 2678 | 1.40 |
CNO 1 | 1341 | 1578 | 2677 | 1.17 |
CNO 2 | 1345 | 1589 | 2688 | 1.41 |
CNO 3 | 1337 | 1576 | 2667 | 1.23 |
CNO 4 | 1341 | 1581 | 2676 | 1.35 |
CNO 5 | 1341 | 1579 | 2676 | 1.16 |
CNO 6 | 1349 | 1596 | 2692 | 1.40 |
CNO 7 | 1342 | 1578 | 2680 | 1.18 |
CNO 8 | 1342 | 1579 | 2680 | 1.61 |
CNO 9 | 1340 | 1578 | 2675 | 1.34 |
CNO 10 | 1342 | 1579 | 2684 | 1.53 |
The intensity ratio ID/IG is observed to decrease after the first step of the reactions (Scheme 1) for CNO 1, CNO 3, CNO 5, CNO 7 and CNO 9. These observations indicate a decrease in the number of sp2-hybridized atoms after the covalent functionalization of CNOs. An increase in the intensity of ID/IG for CNO 2, CNO 4, CNO 6, CNO 8, and CNO 10 results from an increase in sp2-hybridized CC bonds in the structure due to the addition of ferrocene to the CNO surface. All samples also exhibit broad 2D bands at approximately 2680 cm−1. The 2D band is an overtone of the D band and is sensitive to changes in the electronic structure of the molecules.40,41
Fig. 3 (a) TGA and (b) DTG curves of pristine CNOs (), CNO 2 (), CNO 4 (), CNO 6 (), CNO 8 () and CNO 10 () under an air atmosphere at 15 °C min−1. |
Sample | Peak | Onset T (°C) | Inflection T (°C) | End T (°C) | Weight loss (%) |
---|---|---|---|---|---|
CNO | 1 | 500 | 633 | 700 | 98 |
CNO 2 | 1 | 176 | 259 | 600 | 89 |
2 | 506 | ||||
CNO 4 | 1 | 100 | 365 | 633 | 91 |
2 | 524 | ||||
CNO 6 | 1 | 112 | 435 | 630 | 94 |
2 | 524 | ||||
CNO 8 | 1 | 100 | 347 | 630 | 92 |
2 | 500 | ||||
CNO 10 | 1 | 100 | 300 | 565 | 78 |
2 | 400 |
The CNO-Fc derivatives start to decompose in the temperature range between 100 and 176 °C. The most intense peaks are observed at 506, 524, 524, 500 and 400 °C for CNO 2, CNO 4, CNO 6, CNO 8 and CNO 10, respectively. The sharp mass-loss transition corresponding to the combustion of CNOs shows that the material is a homogeneous single phase with very few impurities. Fig. 4a reveals that CNO 2 and CNO 10 have the highest degree of CNO surface functionalization (Table 2).
Fig. 4 UV-vis spectra of (a) Fc-COOH, (b) CNOs, (c) CNO 2, (d) CNO 4, (e) CNO 6, (f) CNO 8 and (g) CNO 10 in ethanol. |
The excited-state properties were examined by steady-state fluorescence measurements to probe the excitation of the donors. Fluorescence spectra were obtained for CNO 2, CNO 4, CNO 6, CNO 8 and CNO 10 (Fig. 5). Since the highest emission of Fc-COOH was observed using 300 nm excitation, the emission spectra of the CNO-Fc derivatives were obtained using this excitation wavelength. The emission intensities of the CNO-Fc derivatives increase in the following order: CNO 6 < CNO 4 < CNO 10 < CNO 8 < CNO 2. These intensities were all higher than that of pristine CNOs. The probability of excited state deactivation by fluorescence for each CNO-Fc derivative was measured and is expressed as the quantum yield, ϕf (Table 3).
Fig. 5 Fluorescence emission spectra of Fc-COOH (), unmodified CNOs (), CNO 2 (), CNO 4 (), CNO 6 (), CNO 8 (), and CNO 10 () in ethanol (photoexcited at 280 nm). |
Sample | E ox (onset) CV vs. Ag/AgCl | E ox (max) DPV vs. Ag/AgCl | λ onset (nm) | HOMOCV (eV) | LUMOopt (eV) | E g (eV) | |
---|---|---|---|---|---|---|---|
a ϕ f quantum yields determined for Fc-COOH and CNO-Fc derivatives in ethanol; , I – integrated fluorescence intensity, OD – optical density, and n – refractive index; subscript ‘r’ refers to the reference fluorophore. | |||||||
Fc-COOH | 0.27 | 0.328 | 0.435 | — | — | — | — |
CNO 2 | 0.74 | 0.288 | 0.385 | 321 | −5.00 | −1.14 | 3.86 |
CNO 4 | 0.52 | 0.327 | 0.425 | 322 | −5.04 | −1.19 | 3.85 |
CNO 6 | 0.22 | 0.320 | 0.420 | 304 | −5.03 | −0.95 | 4.08 |
CNO 8 | 0.62 | 0.322 | 0.425 | 324 | −5.03 | −1.20 | 3.83 |
CNO 10 | 0.59 | 0.180 | 0.635 | 321 | −4.89 | −1.03 | 3.86 |
The highest quantum yield was observed for CNO 2, and the lowest for CNO 6. On the basis of the ϕf values and the UV-vis absorption spectra, it is concluded that the introduction of the best chromophore does not lead to the highest ϕf (Table 3). Therefore, the fact that the functionalization of CNOs may proceed with different yields is a consequence of not only different synthetic routes but also steric effects between donor groups on the surface.
Diffuse reflectance spectroscopy (DRS) was used to monitor the reflectance of the CNO and CNO:P3HT layers in solid phase (Fig. SI1†). This method is used for the characterization of chromophores, which are too opaque to permit the conventional use of UV-vis spectroscopy.50,51 The CNO and CNO:P3HT layers were studied by DRS in the range between 280 and 850 nm (Fig. SI1†). For both layers we observed interaction of light with the CNOs and CNOs:P3HT up to 850 nm (Fig. SI1†). Apparently, the reflectance of the chromophores has a different characteristics in solution and solid phase.50,52 Usually, if the physical adsorption (van der Waals interaction) occurs, the following differences between transmittance and reflectance are observed: the reflectance spectrum is broadened, the bands are displayed toward longer wavelengths, the vibrational structures is strongly suppressed, frequently appearing as a broad humps.52 Additionally, the active layers are very sensitive to every parameters during the film formation (temperature, solvent annealing, the weight ratio of components, aggregation of nanoparticles, thickness of the active blend layer, etc.).53 All the complementary features of the absorption bands of the CNO and CNO:P3HT layers broaden the light-harvesting wavelength range of these blends in their solid phase (Fig. SI1†).
Fig. 6 shows the CV (Fig. 6, panel (I)) and DPV (Fig. 6, panel (II)) plots for the compounds. In addition, Table 3 summarizes the measured potentials as determined by CV and DPV. The measurements were performed in an acetonitrile/toluene (ACN/tol) mixture (1:4, v/v) with 0.1 mol L−1 TBAPF6, as the supporting electrolyte, at 25 °C and at a scan rate 50 mV s−1 under an argon atmosphere. All products originating from the CNO-Fc derivatives and their ferrocene reference compounds show electrochemically reversible first oxidation waves (Fig. 6, panel (I)). The Ox1 and R1 peaks observed for the CNO-Fc systems (CNO 2, CNO 4, CNO 6, CNO 8 and CNO 10) correspond to the reversible one-electron oxidation-reduction of iron67 and to diffusion-controlled Fc/Fc+ oxidation.54,55
The compounds containing ferrocenyl groups show a one-electron oxidation process at potentials that vary little with the spacer group between the CNO core and the Fc moiety.54 Furthermore, the redox properties of hybrids CNO 2, CNO 4, CNO 6, CNO 8 and CNO 10 are different from those of the model compounds CNO 1, CNO 3, CNO 5, CNO 7 and CNO 9, respectively. When comparing the behaviour of Fc-COOH to that of CNO 2, CNO 4, CNO 6 and CNO 8, the oxidation potential clearly shifts from +0.44 V to more negative potentials, reflecting the acceptor property of the CNOs (Fig. 6, panel (II)). The scan of CNO 10 is different from that of the other ferrocene derivatives, as shown in Fig. 6h. DPV shows that the oxidation peak is shifted anodically to +0.64 V (vs. Ag/AgCl) compared to the +0.54 V of the Fc-P model.
The electronic/optical energy level (Eg) is a key parameter of conjugated photosensitive structures. Eg values can be calculated from the electrochemical measurements or from the absorption spectra, by subtracting the highest occupied molecular orbital (HOMO) and lowest unoccupied molecular orbital (LUMO) energies.
The HOMO energy levels of the CNO-Fc derivatives were estimated from the onset oxidation potential of the first peak (Eox(onset)) obtained from the CVs, based on eqn (1):
HOMO = −(Eox(onset) + C) (eV) | (1) |
LUMO = HOMO + Eg (eV) | (2) |
(3) |
The calculated HOMO and LUMO energy levels are collected in Table 3. The electrochemical HOMO energy levels (calculated using eqn (1)) of the CNO-Fc derivatives are between −4.89 eV (CNO 10) and −5.04 eV (CNO 4) (Table 3). The optical LUMO energy levels (calculated using eqn (2) and (3)) of the CNO-Fc derivatives are between −0.95 eV (CNO 6) and −1.20 eV (CNO 8). The HOMO energy levels of the CNO-Fc derivatives are dominated by the ferrocene group, and the LUMO energy levels of the CNO-Fc derivatives are centered on the carbon cages. Thus similar band gaps of ∼3.85 eV are obtained for CNO 2, CNO 4, CNO 8 and CNO 10. The lowest value of Eg = 3.85 eV and the highest value of Eg = 4.08 eV are obtained for CNO 4 and CNO 6, respectively, and are consistent with the results obtained from the steady-state fluorescence measurements (Table 3).
(4) |
The morphology and interfacial behaviour of the multicomponent active layer confined between the electrodes are influenced by the preparation conditions and solubilities of the photoactive compounds.74 The morphology and roughness of each layer of the OPV cell were studied by scanning electron microscopy (SEM) for CNO 4 as part of the active layer (Fig. SI2†). The SEM images at different magnifications of the ZnO layer are shown in Fig. SI2a–c.† The surface of ZnO is perfectly flat and homogeneous, and consequently, it is a great foundation for the active layer of the OPV (Fig. SI2†). The morphology of the P3HT:CNO 4 layer (Fig. SI2d–f†) differs significantly from the morphology of thin films of ZnO (Fig. SI2a–c†) due to unevenness of the surface, which results from the nature of CNOs and their aggregation properties. Nevertheless, the dispersibility of CNOs in polar and non-polar solvents also strongly depends on their functionalization. Homogenous distributions of CNO particles are obtained for all CNO derivatives except for CNO 6, which shows low dispersibility in o-DCB.
For all OPV devices we used the same mass concentration of the CNO derivatives (8 mg mL−1 in a P3HT:CNO-Fc dispersion). The CNOs and their derivatives have a limited dispersibility in all solvents. The nitrogen adsorption studies indicated that CNO 4 had the highest value of the pore volume and additionally showed the highest dispersion in o-DCB. These two factors should have a significant positive impact on the OPV performance parameters. The extended absorption of sunlight at longer wavelengths directly reflects on the value of Jsc,75,76 and a higher current density was achieved (Fig. SI3† and Table 4).
Acceptor | J sc (mA cm−2) | V oc (V) | FFb (%) | PCE (%) |
---|---|---|---|---|
a The calculated short circuit current values were obtained from the external quantum efficiency curves (Fig. SI3) using the correlation . b The calculated FF were obtained using equation FF = Pmax/VocJsc with Jsc calculated as shown.a | ||||
CNOs | 3.07 | 0.08 | 22 | 0.05 |
CNO 2 | 7.51 | 0.17 | 40 | 0.51 |
CNO 4 | 10.66 | 0.35 | 49 | 1.89 |
CNO 6 | 3.67 | 0.09 | 23 | 0.08 |
CNO 8 | 6.80 | 0.14 | 35 | 0.33 |
CNO 10 | 7.85 | 0.23 | 40 | 0.72 |
The current density–voltage (I–V) characteristics of all CNO derivatives used as components of the active layer in OPV devices are shown in Fig. 7. All measurements were done under illumination equal to AM 1.5 G (100 mW cm−2) at a current density in the range between ca. 3 and 11 mA cm−2. Using the measured external quantum efficiency (EQE) data Jsc was calculated under 100 mW cm−2 of AM 1.5 G solar irradiation, according to the formula:
(5) |
The highest PCE equalling 1.89% was obtained with an open-circuit voltage of 0.46 V (Voc), a Jsc of 10.66 mA cm−2 (calculated from the EQE curves, Fig. SI3†) and a fill factor of 49% (FF) for the CNO 4-based device. The Jsc of the BHJ solar cells for all five CNO-Fc derivatives range from 3.67 to 10.66 mA per cm2 and the FF values from 23 to 49%. The device constructed with non-modified CNO shows a PCE value of 0.05% (Jsc = 3.07 mA per cm2, Voc = 0.09 V, and FF = 22%). The lowest PCE value (0.08%), Voc (0.10 V), and FF (23%) was observed for the device in which P3HT:CNO 6 is used as the active layer. These values are strongly correlated with the high aggregation of this derivative in solution. Experimental evidence shows, that the PCE of these devices is improved by functionalization of the CNOs, which decreased the CNO's Eg and increased their dispersibility.
However, the obtained PCE results are still far from the values of other OPV devices with incorporated CNs, where these nanostructures were used as a light harvester or as charge transporters (Table 5). It has to be underlined that CNOs are used as an acceptor' in our OPV cells.
Devices | PCE (%) | Note | Ref. |
---|---|---|---|
a Abbreviations: PEDOT – poly(3,4-ethylenedioxythiophene); BCP – bathocuproine; PDDA – poly(diallyldimethylammonium chloride); P3HT – poly(3-hexylthiophene); PCBM – [6,6]-phenyl-C61-butyric acid methyl ester; PVBTAn+ – poly[(vinylbenzyl)trimethylammonium chloride]; ZnP8− – Zn porphyrins; PTB7 – polythieno[3,4-b]thiophene/benzodithiophene; PC71BM – [6,6]-phenyl-C71-butyric acid methyl ester; N-CNT – nitrogen-doped carbon nanotubes; ICBA – indene-C60 bisadduct; QD – quantum dots; B-MWNT – boron-doped multi-walled carbon nanotubes; Bphen – bathophenanthroline. | |||
Pristine without dopants | |||
ITO/PEDOT/SWNT:P3HT/BCP/Al | 0.72 | Using semiconducting SWNTs coated with P3HT | 56 |
ITO/ZnO/P3HT:SWNT/MoS2/PEDOT/Au | 0.46 | SWNTs enabled a mixture of MoS2 and P3HT | 57 |
ITO/PEDOT/CNT:P3HT:PCBM/LiF/Al | 2.00 | — | 58 |
ITO/PDDA/SWNT–PVBTAn+/ZnP8− | 3.81–9.90 | For covalent and non-covalent functionalization of SWNTs with PVBTA | 59 |
ITO/ZnO/CNO 4:P3HT/Ag | 1.89 | — | This work |
With dopants | |||
ITO/PEDOT/SWNT/C60/Ag | 0.46 | — | 60 |
ITO/PEDOT:PSS/MWNT:C60/Al | 0.80 | — | 61 |
ITO/PEDOT/PTB7:PC71BM:N-CNT/Ca/Al | 8.60 | — | 62 |
ITO/PEDOT/P3HT:ICBA:QD:N-CNT/TiOx/Al | 6.11 | QDs were used to enhance doping and dispersion | 63 |
ITO/PEDOT/P3HT:PCBM:B-MWNT/TiOx/Al | 4.10 | B-MWNTs were used to enhance PCE | 64 |
ITO/PEDOT:PSS:CNO/perovskite/PCBM/Bphen/Ag | 15.26 | — | 32 |
Several examples of OPV devices containing CNs as dopants are presented in Table 5. Systems similar to our OPV devices, with single-walled carbon nanotubes incorporated in an active layer, provided a PCE of ca. 1% (Table 5). One of the highest PCE values was obtained by Prato and co-workers for the SWNT–poly[(vinylbenzyl)trimethylammonium chloride] (PVBTAn+).59 SWNT–PVBTAn+ was synthesized by the free-radical polymerization of (vinylbenzyl)trimethylammonium chloride. PVBTAn+ was also noncovalently wrapped around SWNTs to form a positively charged SWNT/PVBTAn+ suspension in water. Photocurrent measurements gave PCEs of 3.81 and 9.90% for the covalently and noncovalently modified SWNTs, respectively. It was already stressed that one of the highest PCE values for OPV devices was obtained for ITO/PEDOT:PSS:CNOs/perovskite/PCBM/Bphen/Ag (Table 5).32 In this system, spherical CNOs were used as dopants in PEDOT:PSS, which reduced the acidity and hydrophilicity of this layer and suppressed the corrosion of ITO.
This comparison shows that the use of larger CNs in OPV devices is also very promising. It should be emphasized that the CNO-Fc derivatives were used to construct one of the simplest OPV systems reported in the literature.
FTIR-spectra were recorded with an FT-IR Nicolet iN10 MX microscope in the range from 4000 to 700 cm−1 using an array detector cooled by liquid nitrogen. The 1H NMR spectra were recorded on a Bruker Avance II spectrometer (400 MHz) at room temperature in deuterobenzene and were referenced to residual solvent peaks. The chemical shifts are represented in ppm. The Raman spectra were collected using a Renishaw spectrometer with a liquid N2-cooled charge-coupled device (CCD) within a range from 3500–100 cm−1 excited by an Ar+ ion laser (514 nm) and a 20× lens. SEM images were recorded with an SEM FEI Tecnai S-3000N microscope 1000× with a resolution of 100 μm. The samples were applied to gold foil and prepared on an aluminium plate.
UV-vis spectra were recorded using a Hitachi U-3900H spectrophotometer equipped with a double monochromator and a double-beam optical system (190–800 nm). Steady-state emission spectra were recorded on a Hitachi F7000 fluorescence spectrophotometer. The measurements were carried out at room temperature. The diffuse reflectance (DR) measurements were made by an elipsometric spectrophotometer SENTECH Instruments GmbH SE850. The spectra were registered in the spectral range between 280–850 nm.
Thermogravimetric experiments were performed using an SDT 2960 with simultaneous TGA-DTG (TA Instruments company). The thermogravimetric traces were recorded at 15 °C min−1 in an air (100 mL min−1).
N2 gas adsorption measurements were performed using a Micromeritics apparatus (ASAP2020 – automatic sorption analyser, Micromeritics Corp., USA) at −196 °C. Prior to the gas adsorption analysis, all samples were degassed at 100 °C and 10 μm Hg vacuum for 20 h to remove any adsorbed species.
Voltammetric experiments were performed using an AUTOLAB (Utrecht, The Netherlands) computerized electrochemistry system equipped with a PGSTAT 12 potentiostat using a three-electrode cell placed in a Faraday cage. The AUTOLAB system was controlled with the Nova 1.10 software from the same manufacturer. A glassy-carbon disk electrode (Bioanalytical Systems, Inc.) with a diameter of 2 mm (Bioanalytical Systems, Inc.) was used as the working electrode. The surface of the electrode was polished using extra-fine carborundum paper (Buehler), followed by 0.3 μm alumina and 0.25 μm diamond polishing compounds (Metadi II, Buehler). The electrode was then sonicated in water to remove traces of alumina from the metal surface, washed with water, and dried. The counter electrode was a platinum square with an area of approximately 0.5 cm2. A silver wire immersed in 0.01 mol L−1 AgCl and 0.09 M TBAClO4 and separated from the working electrode by a ceramic tip (Bioanalytical Systems, Inc.) served as the reference electrode. The active material (CNO 1–CNO 10 and their ferrocene references) with a concentration 0.5 mg mL−1 was suspended in an acetonitrile and toluene mixture at a volume ratio 1:4 with 0.1 mol L−1 TBAPF6 as the supporting electrolyte. Oxygen was removed from the solution by purging with argon.
The J–V curves were measured using solar simulator Model #SS50AAA PET from Photo Emission Tech, Inc. with a Keithley 2401 source-meter. The lamp emitted standardized sunlight, whose spectrum of radiation was close to a spectrum of an air mass 1.5 global AM (1.5 G) irradiation. Additionally, an atmospheric correction was used, assuming that all measurements were made at 25 °C and at a standard radiation intensity of 100 mW cm−2. The solar simulator was calibrated using a reference silicon solar cell.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c9na00135b |