Takashi
Tsuji
,
Kenji
Hata
,
Don N.
Futaba
* and
Shunsuke
Sakurai
*
CNT-Application Research Centre, National Institute of Industrial Science and Technology (AIST), Central 5, 1-1-1, Higashi, Tsukuba, Ibaraki 305-8565, Japan. E-mail: d-futaba@aist.go.jp; shunsuke-sakurai@aist.go.jp
First published on 2nd September 2019
Here, we demonstrate an approach of increasing the density of ultralong carbon nanotube (CNT) growth by combining a fast-heating method developed by Huang et al. (J. Am. Chem. Soc., 2003, 125, 5636–5637) with catalyst support engineering. Specifically, using graphene oxide as a catalyst support for iron oxide (Fe3O4) catalyst nanoparticles, we achieved high density growth of CNTs grown by the “kite-mechanism”. Our analysis revealed that the fast-heating method reduced undesired aggregation of the catalyst nanoparticles, which has been reported to be a primary limitation mechanism, by shortening the time between substrate heating and CNT growth. In addition, the use of the graphene oxide support led to controllable and uniform dispersion of catalyst nanoparticles in relatively high density which provided increased process control by extending the time before the onset of catalyst aggregation. Together, these approaches suppressed the aggregation of the catalyst nanoparticles, which facilitated the “tip-growth” mode instead of the “root-growth” mode, and led to the high density growth of ultralong CNTs. Our results also indicate additional limitations and complexities on the high density CNT growth by the kite-growth approach, which limit high density synthesis.
Although much progress has been made on growing ultralong CNTs by this gas-flow directed CVD, increasing the growth efficiency in terms of CNT number density remains a challenge. The typical density of the ultralong CNTs is only several CNTs/100 μm where only a few CNTs are successful in growing ultralong across a 100 μm wide region of catalyst nanoparticles, and the highest reported density was 60 CNTs/100 μm by Liu et al.9 This is in stark contrast to highly dense (∼103–104 CNTs only in the 1 μm2 catalyst region) CNTs grown from substrates based on the “root-growth” or “base-growth” mechanism which have shown catalyst activities as high as 84%.10
One of the primary causes of low CNT density, i.e. catalyst activity, in kite-growth is thought to be the formation of aggregated large catalyst nanoparticles. Since large nanoparticles tend to grow CNTs with the catalysts “rooted” to the surface,11 the mobility of particles on the catalyst support accelerated at the high process temperature can disable kite-growth. The previously reported process of gas-flow directed CVD consisted of (1) catalyst deposition on a substrate (usually SiO2), (2) reduction of the catalyst nanoparticles (usually by heating in a hydrogen (H2) environment for a few minutes), and finally (3) CNT growth. The highest values of CNT number density were obtained by optimization of the above process. Specifically, Liu et al. reported 60 CNTs/100 μm by optimizing the catalyst deposition method (post-annealing of Fe after deposition),9 and Zhou et al. obtained 20–30 CNTs/100 μm by optimizing a copper catalyst.12 However, it is fundamentally difficult to avoid catalyst nanoparticle aggregation in the above process because of the high mobility of metal catalyst nanoparticles on SiO2 surfaces at a high temperature range.
Catalyst support engineering and the fast-heating process are two approaches to overcome the above problem in the previous research. Since the interaction between the catalyst and the catalyst support layer plays an important role in the stability of catalyst nanoparticle arrays for root-growth systems,13–16 a number of approaches have similarly employed “catalyst support engineering” on kite-growth. For example, the use of silica nanospheres17 or graphene/graphite sheets18 has shown suppression of catalyst aggregation, which resulted in improved number density of ultralong CNTs compared to the commonly used SiO2 support (∼3 CNTs/100 μm17), but not exceeding the highest value of kite-growth. The fast-heating method, developed by Huang et al.,1,19 is one of the methods particularly suitable for gas-flow directed CNT growth. In this method, the catalyst-coated substrate is rapidly transferred into a preheated reactor already set at the CNT growth environment. As a result, the exposure time of catalyst particles to a high temperature environment is drastically shortened, thus reducing the probability of catalyst aggregation. Huang et al. grew ultralong CNTs by using several varieties of catalysts, such as iron/molybdenum (Fe/Mo) nanoparticles, iron/platinum nanoparticles, Fe/Mo molecular clusters and carbon sources, such as carbon monoxide (CO), methane (CH4) or methanol.1 Although the number density of the ultralong CNT was not mentioned in the report, estimation of the CNT density from the published images appears to be below 1 CNT/100 μm in most cases with a maximum of 7–8 CNTs/100 μm (in the case of the Fe/Mo catalyst and CO carbon source). Taken together, these results indicate that the use of the fast-heating method alone or catalyst support engineering alone is not sufficient to grow high density CNTs.
In this study, we have combined the use of the fast-heating approach with catalyst support engineering as a method to increase CNT number density. Specifically, using iron oxide (Fe3O4) nanoparticles cast with graphene oxide (GO) support as catalysts, the density of ultralong CNTs grown by the fast-heating method reached ∼20 CNTs/100 μm. While not the highest reported, this value compares well with that reported by Liu et al.9 and Zhou et al.12 The graphene oxide allowed for well-separated catalyst nanoparticles across the surface and the fast-heating process facilitated the CNT growth before significant catalyst aggregation occurred. Combination of these effects led to the high density growth of ultralong CNTs. Our results further show that the achievement of high density CNT growth by a kite-mechanism is highly complex and only begins with the preparation of suitably spaced and active nanoparticles, followed by a suppression in the interaction between growing nanotubes.
In order to understand the importance of the fast-heating method, we examined the effect of the timing of the carbon source delivery on the CNT number density. Specifically, we modulated the “delay time” between the moment the sample reached the center of the furnace and the time the gas flow, containing carbon source, reached the sample position (see ESI 3† for a detailed definition). Number densities of CNTs estimated by SEM images (Fig. 2a–d) were plotted as a function of this “delay time” (Fig. 2e). As a whole, the trend of the CNT densities resembled an inverse S-curve shape characterized by (1) a region of high CNT density, (2) a region of decreasing CNT density, and (3) a region of no CNT growth. In the high CNT density region (<10 s), the numbers of observed CNTs were found to be the highest (Fig. 2a). The second region (beginning at ∼10 s) was characterized by a sharp decrease in the CNT density. Finally, in the no CNT growth region, CNT number density approached zero. Importantly, the window of the high CNT density region (∼10 s) was estimated to be comparable to the heating time for the catalyst to reach the reactor temperature (900 °C). When a thermocouple probe was inserted into the furnace at a speed similar to that of the actual substrate (∼10 mm s−1) as a simple test, a further ∼15 s was required for the probe temperature to reach 900 °C from ∼700 °C, the value when the probe reached to the center of the furnace. The result clearly shows the necessity of the catalyst nanoparticles to react with the carbon source and start the CNT growth within a particularly short time after the substrate/catalyst reaches growth temperature for achieving a high density growth of the ultralong CNTs.
We used transmission electron microscopy (TEM) and AFM to investigate the evolution of the catalyst nanoparticles in the CVD process environment. A silicon nitride membrane grid with micropores was immersed into the aqueous solution of 5 nm Fe3O4 nanoparticles and the GO for 10 min. ∼5 nm particles supported on the GO layers covering the microporous region were observed (Fig. 3a and S3†). The TEM grid was then transferred to the CVD reactor preheated at 900 °C and kept only for 6 s in H2 using the fast-heating method. TEM observation showed a reduction in catalyst number density and an increase in size (∼13 nm on average) by this fast-heating (Fig. 3b). Similarly, a Fe3O4/GO catalyst-coated SiO2/Si substrate was also heated at 900 °C in a H2 environment for a set time (6, 30, and 180 s) and observed by AFM. AFM observation (Fig. 3c–f) also showed the increase of particle size with heating time. These results further indicate the relatively high rate at which the catalyst nanoparticles coarsen by enhanced particle movement on the GO support due to the high process temperature, which is in agreement with the CNT density delay time results of Fig. 2. Importantly, these results clearly show the importance of the fast-heating method for suppressing catalyst aggregation during the H2 reduction.
To demonstrate the importance of using the GO support, the Fe3O4 nanoparticle catalyst, alone, was deposited without using the GO support, and then subjected to the fast heating CVD process. Significantly decreased CNT number density (∼2 CNTs/100 μm) was observed in this case (Fig. 4a). This result indicates the critical role of the GO support in increasing the number density of grown CNTs by nearly 10-times (∼20 CNTs/100 μm) as shown in Fig. 1c likely by forming a well-separated array of Fe3O4 nanoparticles.
To investigate the role of GO in the separation of catalyst nanoparticles, a comparative SEM observation of the catalyst systems with and without GO was performed after the growth process. In the case where the Fe3O4 catalyst, alone, was deposited onto the SiO2/Si substrate, extremely coarsened aggregates with a size of ∼1 μm were observed in large numbers (Fig. 4b). In stark contrast, the SEM image of the Fe3O4/GO system showed no large micrometre-scale particles, but rather a large number of smaller particles and many entangled CNTs (Fig. 4c). Taken together, these results provide clear evidence of the ability of the GO support for a well-separated Fe nanoparticle array after coating and even after heating up to the CNT growth environment.
As mentioned previously, large nanoparticles formed by aggregation tend to grow CNTs by a “root-growth” mode instead of a “tip-growth” mode, resulting in short MWCNTs. Both the fast-heating method and the use of the GO support facilitated the CNT growth before substantial catalyst coarsening could occur. Our results showed that the fast-heating method shortened the necessary catalyst reduction time prior to the growth step, thus reducing the time for catalyst aggregation to occur. In addition, use of GO as the catalyst support improved the dispersibility of the catalyst nanoparticles, thus increasing our process control by extending the allowable window of time between substrate insertion and carbon feedstock contact. In doing so, the initiation of CNT nucleation before catalyst aggregation improved the number density of the ultralong CNTs. It should be noted that direct comparison using neither the fast-heating method nor GO support resulted in no observable CNT growth under our experimental conditions (Fig. S4†). This result shows the significance of the collective effects of the fast-heating method and the use of GO supports.
Finally, we recognize that despite our approach of using a fast-heating method and catalyst engineering (such as the GO catalyst support) to increase the obtained CNT densities, we were unsuccessful in achieving higher densities than previously reported ones. Specifically, modulation of the Fe3O4 concentration did not show any significant changes in the grown CNT density (10–20 CNTs/100 μm, Fig. S5†). We believe our results to be general to other catalyst systems as similar results were obtained using a catalyst support composed of an aggregate of the as-grown CNTs (e-DIPS CNTs). The observed CNT number density was estimated to be 22 CNTs/100 μm (Fig. 5). Importantly, despite the extreme structural difference in these two catalyst/support systems, the resulting number density of grown CNTs converged to the similar values of ∼20 CNTs/100 μm.
The above results suggest that the number of ultralong CNTs, in our experiments, is not limited by the number of catalysts which nucleate the tip-growth, which indicates that increasing the density of flying CNTs represents a more complex process which extends beyond the suppression of catalyst aggregation and catalyst–support interaction. Analogous to the formation of a CNT forest, which requires a combination of a growth environment supporting a high catalyst activity,10 appropriately spaced catalyst nanoparticles based on their size,21 and stable catalyst array13 to ensure vertical growth, the achievement of kite-growth CNTs also requires a strict set of conditions. Further, the interaction between CNTs adds to the complexity. Therefore, from our results, we propose that the following steps are additionally necessary for high density kite-growth CNTs in a single growth: (1) liftoff and (2) sustained buoyancy for extended lengths.
First, liftoff is defined as the moment the catalysts leave the substrate surface and begins the kite-growth process. This step is particularly complex as the growth directionality in the early stages of growth is largely random as observed (Fig. 4c), which results in collisions and entanglements among neighboring CNTs. Our observations strongly indicate that this is another severe bottleneck in achieving high density, which would require either large catalyst spacing or unidirectional growth. Second, sustaining the buoyancy for extended growth represents another obstacle for high density growth. In short, entanglements between highly-dense CNTs in the gas flow will act to disrupt the buoyant forces necessary for kite-growth. In experiments presented here, we observed many entangled CNTs in our samples just outside the catalyst region and after the liftoff step, as shown in Fig. 1c. Therefore, as outlined above, although an array of stable and catalytically active nanoparticles is an important first step to increase the density, limiting intertube entanglements just after liftoff remains a significant obstacle. Resolving the entanglement during and after liftoff remains a significant issue, and we expect that our work will facilitate future work to address these issues.
Growth of CNTs was performed using an automated 1-inch horizontal quartz tube using the fast-heating CVD process. The substrate put on the quartz holder was transferred into the furnace preheated at 900 °C with a speed of 10 mm s−1 in an environment of H2:CH4 = 1:1 (total flow: 1000 sccm) and then kept for 10 min.
Characterization of the grown CNTs and the catalyst was performed using a SEM (Hitachi, S-4800), AFM (Bruker, Dimension FastScan) and Raman spectrometer (Thermo Fisher Scientific, NICOLET ALMEGA XR) with 532 nm excitation. The Raman spectrum was obtained from the suspended segments of CNTs across a trench in a SiO2/Si substrate shown in Fig. S2.† The trenches on silicon wafers were fabricated using a laser with ∼100 μm in width and ∼63 μm in depth. TEM (TOPCON EM-002B) was used to observe Fe3O4 nanoparticles on GO flakes. A silicon nitride membrane grid with 2 μm micropores (SN100-A20MP2Q05, ALLIANCE Biosystems) was first immersed into an aqueous solution of 0.1 vol% (3-aminopropyl)triethoxysilane (Wako) for 30 min and rinsed with water. After drying (105 °C, 30 min, in air), the grid was immersed into the aqueous solution of 5 nm Fe3O4 nanoparticles and GO for 10 min. Then the grid was rinsed in pure water then ethanol and finally dried in air (105 °C, 1 hour).
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c9na00209j |
This journal is © The Royal Society of Chemistry 2019 |