Zhiming Wangab,
Yuning Sun*ab,
Shuo Zhanga and
Yonglong Wanga
aSchool of Energy Science and Engineering, Henan Polytechnic University, Jiaozuo, 454002, China. E-mail: sunyn639@126.com
bState and Local Joint Engineering Laboratory for Gas Drainage and Ground Control of Deep Mines, Henan Polytechnic University, Jiaozuo, 454000, China
First published on 29th March 2019
In this investigation, sodium silicate (SS) was mixed into rich-water (RW) materials consisting of Portland cement, calcium aluminate cement and gypsum for improved mechanical properties. The RW materials containing different amounts of SS were characterized by the compression test, mercury intrusion porosity, scanning electron microscopy, X-ray diffraction and Fourier transform infrared spectroscopy. The results demonstrated that with the increase of SS additions, the early strength of the RW materials increases, and the long-term strength retrogression of the RW materials can be inhibited when the SS content is above 3%. Pore structures of the RW materials are improved significantly due to the filling effect of the calcium silicate hydration (C–S–H) gel from a reaction between silicate ions and Ca(OH)2, thus increasing the early strength of the RW materials. For the RW materials containing SS and cured for 0 to 14 days, there are more hexagonal hydrates including CaO·Al2O3·10H2O (CAH10) and 2CaO·Al2O3·8H2O (C2AH8), more C–S–H gel and less ettringite crystals, which is of benefit to the strength of the material. The strength retrogression can be attributed to phase conversions from hexagonal hydrates (CAH10 and C2AH8) to cubic ones (3CaO·Al2O3·6H2O) with lower intercrystal bonding forces. Furthermore, this phase conversion is inhibited effectively by the chemical reaction of silicate ions and CAH10 (or C2AH8), improving the long-term strength of the RW materials.
Portland cement (PC) has been produced widely in the world, with low cost and rich resources. However, straight PC is not an ideal material to prepare the grouting slurry due to its long setting time, low early strength and obvious shrinkage at a high value of W/S.5 For CAC, high early strength is one of the major advantages. Besides, the CAC has other advantages of short setting time, chemical aggression resistance and high temperature resistance.6 However, because of the crystalline conversion from the metastable hexagonal CaO·Al2O3·10H2O (CAH10) or 2CaO·Al2O3·8H2O (C2AH8) to cubic 3CaO·Al2O3·6H2O (C3AH6), the porosity of CAC paste increases and the long-term strength decreases markedly as a consequence.7 Meanwhile CAH10 or C2AH8 can react with calcium silicate hydrate (C–S–H) gel to produce 2CaO·Al2O3·SiO3·8H2O (C2ASH8), which is dependent on the availability of C–S–H gel during this reaction process.6–8 To obtain advanced materials with short setting time, good strength and low cost, PC and CAC are usually mixed to form PC–CAC binary system.9–12 At W/S < 0.6:1, when the mass proportion of PC is 5%, the early strength of PC–CAC binary system is improved, and no long-term strength reduction is detected; and when the proportion of PC is 20%, the long-term strength decreases significantly.9 And, when the mass ratio of CAC is 20%, the early strength of PC–CAC binary composite material is higher than that of pure PC, and the strength rises over time.11 In addition, it was reported that there is an enhancement on the strength of materials consisting of PC or CAC after the addition of sodium silicate (SS).13–15
The studies mentioned above provide some important guidance to the novel PC–CAC binary composite materials at low values of W/S. However, there were few studies conducted under rich-water conditions (W/S > 1:1). Our prior experimental results have shown that the long-term strength of the rich-water (RW) material composited of PC, CAC and gypsum at relatively high W/S values decreases over time.16 In the present study, SS was mixed to improve the mechanical properties of the RW material at the W/S value of 1.2:1, and the effects of SS on the RW material were investigated. We tested the compressive strength of RW materials containing different amounts of SS. Whilst, the mercury intrusion porosity (MIP), scanning electron microscopy (SEM), X-ray diffraction (XRD) and Fourier transform infrared spectroscopy (FT-IR) were employed to characterize the microstructures of RW materials. Finally, the strength evolutionary mechanism of the RW material was discussed, which could contribute to the future study on this sort of material.
Material | Oxides (wt/%) | |||||||
---|---|---|---|---|---|---|---|---|
CaO | SiO2 | Al2O3 | SO3 | Fe2O3 | K2O | MgO | Na2O | |
PC | 61.67 | 21.75 | 5.57 | 2.36 | 3.58 | 0.87 | 2.21 | 0.43 |
CAC | 37.4 | 0.25 | 61.4 | 0.06 | 0.30 | — | — | 0.27 |
Gypsum | 26.73 | 18.56 | 6.37 | 28.52 | 2.37 | 0.51 | 1.42 | — |
The experimental program is based on the study of four designs of the hardened RW paste. Mass proportions of PC, CAC and gypsum in RW are fixed at 65.5%, 14.5% and 10%, respectively. SS, as an additive blended in the RW material, accounts for 0, 1%, 2%, 3% and 4% of the total mass of the RW material, respectively.
According to GB/T 1346-2011, at W/S of 1.2:1, the paste was stirred twice in a slurry agitator.17 The paste was casted into hollow cylinder moulds (radius of 50 mm and height of 100 mm), and demoulded after 24 hours to prepare cylindrical samples. All the cylindrical samples were cured at (20 ± 2) °C and humidity of (60 ± 5)% until they reached the test ages (3 day, 7 day, 14 day and 28 day).
pd = −4σcosθ | (1) |
MIP tests were conducted in an AutoPore IV 9505 porosimetry (U.S.), whose applied pressure ranges from 0 to 228 MPa and measurable diameter of pore is 5 nm to 1000 μm. Cubic specimens (2.5 × 2.5 × 2.5 cm) sliced from the undamaged cylindrical samples that cured for 3 days, 14 days and 28 days, were prepared. Then, the cubic specimens were dried in a vacuum-oven at a low temperature of 30 °C. This temperature selected was to avoid damaging the microstructure of the samples.
Adopting X-ray diffractometer (D8 Advance, Bruker, Germany) with a 35 kV, 50 mA copper anode X-ray tube and a Cu Kα radiation, the fine powder was examined to determine the hydration products in different ages. Scanning was conducted between 5° and 55° with a 2θ increment of 0.02° s−1.
The fine powder (2 mg) for FT-IR analysis was mixed with dry KaBr powder (200 mg), and driven into disks. The infrared spectra of the disked powder were recorded by VERTEX 70 Fourier transform infrared spectrometer (Bruker, Germany) in the region from 4000 cm−1 to 400 cm−1 at a resolution of 4 cm−1. And the powder was scanned 32 times. To eliminate the impact of vaporous water and carbon dioxide in the spectrometer, we collected the spectrum before putting the sample in the sample cell, which is background spectrum indicating the infrared absorption of the vaporous water and carbon dioxide in the spectrometer. By subtracting the background spectrum, the real spectra of the samples could be obtained. Further, the variations of bonds can be analyzed by peak areas of FT-IR.22–24 In this paper, the peak areas were calculated by peak-differentiating-fitting method combined with Gauss equation. The peak-differentiating-fitting method includes a process of baseline finding-creating, baseline subtracting, peak finding, peak fitting and peak area calculating. What's more, it is required that the correlation coefficients of fitting and experimental curves should be above 0.90.
Fig. 2 Compressive strength of RW materials with SS additions of 0, 1%, 2%, 3% and 4%. All the samples are cured for 3 day, 7 day, 14 day and 28 day, respectively. |
For the RW materials with SS contents of 0, 1% and 2%, their compressive strength decreases during 14 day to 28 day. However, this kind of strength retrogression reduces with the increase in the content of SS. Until the content of SS increases to 3% at least, compressive strength retrogression does not appear during 14 day to 28 day, indicating that the long-term strength retrogression of the RW material can be inhibited effectively by raising the mixing amount of SS.
Fig. 3 Differential pore size distributions of RW materials with SS mixing amounts of 0, 1% and 4%. (a) Curing time of 3 day. (b) Curing time of 14 day and (c) curing time of 28 day. |
On 3 day of hydration and for the hardened RW paste containing no SS, the most probable pore diameter that corresponding to the peak is about 619 nm. And, for the RW materials containing SS of 1% and 4%, the most probable pore diameters are about 552 nm and 516 nm, respectively. It indicates that the pore structure of the RW materials can be improved significantly by mixing SS at early hydration stage. After 14 day's hydration, the most probable pore diameters are 530 nm, 425 nm and 414 nm corresponding to the RW materials containing SS of 0, 1% and 4%, respectively. When curing period of 28 days, the most probable pore diameters of the RW materials are 486 nm, 408 nm and 401 nm corresponding to SS content of 0, 1% and 4%, respectively. Therefore, the difference in the most probable pore sizes of the RW materials between blending with SS and mixing no SS is notable. However, the most probable pore sizes are close for the RW materials containing SS of 1% and 4%. What's more, the difference in the most probable pore size of the RW materials between blending 1% SS and 4% SS reduces over time.
For a further illustration of microstructures of the RW materials and a verification of the MIP results, the micromorphology of the RW materials cured for 3 days and 28 days is shown in Fig. 4. An overview-SEM image at a magnification of 200 is plotted in Fig. 4a, indicating that the chosen areas are representative. And, Fig. 4b shows the SEM images at a magnification of 4000. On 3 day, the number of needle-shaped crystals of the RW paste without SS is more than that of the RW material with SS content of 4%; and for the RW pastes containing SS of 1% and 4%, the pores are filled by amorphous C–S–H gel, leading to a lower porosity. On 28 day, the numbers of the needle-shaped crystals both decrease for the RW materials with and without SS, and the pores are filled by the C–S–H further. Besides, the pore size of the RW material without SS is larger than that of the RW material containing SS of 4%, which is in agreement with the experimental results of MIP.
Fig. 5 XRD patterns of RW materials hydrated for 3 day, 14 day and 28 day. (a) SS addition of 0. (b) SS addition of 1%. (c) SS addition of 4%. (a: AFt, b: CAH10, c: CH, d: CaSO4·2H2O, e: C3AH6, f: CA2, g: C2S, h: C3S, i: AFm, j: CA, k: AH3, l: C2ASH8) When SS content is 1%, the categories of the hydration products on 3 day are the same with those of the RW materials containing no SS. However, the diffraction signal of AFt is much lower, illustrating that the hydration process of CAx is delayed by mixing SS, and this finding agrees with Ding (1995, 1996).32,34 When hydrated for 14 day, the diffraction intensity of CH is lower than the material without SS; and there appear diffraction peaks at d = 11.75 Å, 6.24 Å, reflecting the formation of C2ASH8. According to the studies carried out by Y. Jeong (2018), L. Xu (2017), M. Okoronkwo (2016) and T. Matschei (2007), C2ASH8 can be also detected at the similar peak positions in the calcium sulfoaluminate–belite cement–gypsum, calcium aluminate cement–Portland cement–anhydrite, Portland–CASH or CASH systems.10,35–37. On 28 day, there appears the diffraction signal of C3AH6, but its diffraction intensity is weaker than that in the RW material without SS. |
When SS content is 4%, compared with the RW materials containing SS of 0 and 1%, the diffraction signal of AFt is the lowest at the same hydrated stages. On 14 day and 28 day, there is no obvious diffraction peak of C3AH6. When hydrated for 28 days, the diffraction intensity of C2ASH8 in the RW material with SS content of 4% is much higher than that of the RW material with SS mixing amount of 1%, revealing much more formation of C2ASH8 in the RW with SS content of 4%.
Further, FT-IR was employed to measure the adsorption bands at characteristic wavelength of chemical bonds that vibrate independently, to determine the chemical compositions of materials and to supplement the XRD results. In Fig. 6, the IR spectra for the RW materials containing different amounts of SS can be divided into a high wave number region (4000–1200 cm−1) and a low wave number region (1200–400 cm−1). In high wave number region, it is detected an O–H stretching vibration at around 3659 cm−1 (W1), indicating the formation of C3AH6;31 at 3642–3644 cm−1 (W2), there appear the O–H vibration bonds induced by CH.38 An adsorptive-water adsorption region can be found at 3441 cm−1 (W3), due to the existence of AFt;38,39 and bending vibration bands that induced by the H2O or OH of CAH10 appear at 1637–1639 cm−1 (W4).31,40 In low wave number region, the adsorption bands at 1102–1116 cm−1 (W5) is caused by the asymmetric vibration of SO42− existed in AFt, and the bending vibrations at around 605–616 cm−1 (W8) are also induced by the bands in SO42−;41 at wave number ranging from 965 cm−1 to 969 cm−1 (W6), there appear stretching vibrations induced by silicate/aluminate-oxide structures;31 and the adsorption bonds around 792–798 cm−1 (W7) are attributed to the symmetric stretching vibration of Si–O–Si.42
Fig. 6 Peak fitting of FT-IR spectra of RW materials containing SS amounts of 0, 1% and 4%. The curing time of the materials is 3 day, 14 day and 28 day. |
Table 2 lists the area percentages of fitted peaks calculated using Origin 8.0, which can reflect the content of minerals to some extent. For the RW materials without SS, the peak area percentages at W2, W3, W5, W6, W8 are 2.92%, 45.26%, 17.99%, 9.44%, and 24.39% on 3 day, respectively. From 3 day to 14 day, there shows an increase trend in the area percentages at W2, W6 and W8, but it decreases in the area percentages at W3 and W5. It indicates the increase of the amount of the O–H bonds in CH and Si/Al–O bonds in C–S–H and the decrease of the amount of AFt, which confirmed the XRD findings. The peak area percentages on 3 day and 14 day are both 0 at W1, indicating no formation of C3AH6; the peak area percentages at W4 are 0 and 12.49% on 3 day and 14 day. However, on 28 day, the peak area percentage at W1 raises to 2.87% and the peak area percentage at W4 reduces to 5.74%, which illustrates the formation of C3AH6 and the decrease of CAH10.
Samples | Curing time | Area percentage/% | |||||||
---|---|---|---|---|---|---|---|---|---|
W1 | W2 | W3 | W4 | W5 | W6 | W7 | W8 | ||
RW | 3 day | 0 | 2.92 | 45.26 | 0 | 17.99 | 9.44 | 0 | 24.39 |
14 day | 0 | 3.07 | 35.83 | 12.49 | 10.36 | 10.73 | 0 | 27.52 | |
28 day | 2.87 | 7.71 | 28.05 | 5.74 | 2.02 | 17.77 | 1.06 | 34.78 | |
RW + 1% SS | 3 day | 0 | 2.04 | 41.94 | 0 | 13.98 | 13.36 | 0 | 28.68 |
14 day | 0 | 2.98 | 31.32 | 9.94 | 9.23 | 17.27 | 1.51 | 31.75 | |
28 day | 2.06 | 3.54 | 25.38 | 6.03 | 3.97 | 20.58 | 2.76 | 35.68 | |
RW + 1% SS | 3 day | 0 | 1.07 | 38.63 | 0 | 13.96 | 13.16 | 0.99 | 32.19 |
14 day | 0 | 1.21 | 28.05 | 5.31 | 6.88 | 22.98 | 1.86 | 33.71 | |
28 day | 0 | 2.04 | 23.74 | 2.95 | 0.76 | 27.14 | 2.85 | 40.52 |
When SS contents of 1% and 4%, compared with the RW materials without SS, the peak area percentage at W2 decreases and that at W6 increases on 3 day, respectively, showing much more formation of C–S–H, due to the reaction (eqn (2)).43 It can verify the porosity lowing induced by the filling effect of C–S–H gel.
CH + SiO32− → C–S–H | (2) |
For the RW material with SS content of 1%, the area percentage at W1 is 2.06% on 28 day, which is lower than that in the RW material without SS. However, when the SS content in the RW material increases to 4%, the area percentages at W1 are all 0 on 3 day, 14 day and 28 day, indicating no formation of C3AH6. Besides, for the RW materials with SS additions of 0, 1% and 4%, the area percentage at W4 decreased from 14 day to 28 day, indicating the consumption of CAH10. These are all consistent well with the XRD results (Fig. 5).
(3) |
(4) |
CAH10 and C2AH8 are meta-stable hexagonal hydrates, and C3AH6 is a stable cubic hydrate.10,11,31 And, the intercrystal bonding force of the hexagonal hydrate is larger than that of the cubic one. Therefore, based on the results of XRD and FT-IR, the conversions of CAH10 and C2AH8 to C3AH6 can explain the strength decline of the RW materials with SS content from 0 to 2%.Besides, at initial hydration phase, when there exists SO42−, CAx will hydrate and produce AFt crystals first (eqn (5)).17 However, excessive formations of AFt at early hydration stage will inhibit the hydration process of calcium silicate type minerals (CSx); then, the formation of C–S–H (gel) decreases to induce a lower early strength of the RW materials.44
(5) |
For the RW material without SS hydrated for 14 day, the diffraction intensity of CH is larger than that on 3 day; besides, the peak area become larger at around 967 cm−1. Thus, it indicated the continuous reaction between CxS and water (eqn (6)) during 3 day to 14 day.45,46
CxS + H2O → C–S–H (gel) + CH | (6) |
During 0 to 14 day, the hydrates, CAH10, C2AH8 and C–S–H (gel) are of benefit to the strength, which can explain the increase in strength of the RW material without SS. However, on 28 day, it can be detected the conversion of CAH10 and C2AH8 to C3AH6, inducing a lower long-term strength of the RW material without SS for the lower intercrystal bonding force of C3AH6. The phase variations in the RW material without SS is plotted in Fig. 8a.
Fig. 8 Phase transformation processes in the RW materials (a) without SS and (b) containing SS. Symbols of ↑ and ↓ represent mass increase and decrease, and * represents new hydrates. |
The variation of hydrates in the RW materials containing SS is plotted in Fig. 8b. Combining with XRD and FTIR results, for the RW materials with SS, the hydration rate of CAx is inhibited to cause a decrease in the formation of AFt;32,34 then, the hydration reaction of CSx and the reaction between SS and CH are both accelerated to produce much more C–S–H (gel) to improve the early strength of the material.15 Due to sulfate ions reducing with further hydration, the CAx minerals reacts with water to form CAH10 and C2AH8, this process is similar with that of the RW material without SS. After that, due to the existence of SS, CAH10 and C2AH8 could react with silicate ions to form the stable phase of C2ASH8 before the conversion from the hexagonal crystal to the cubic one (eqn (7)),32 which was also reported by M. Heikal (2017) and J. M. Mercury (2007).6,17 Then, the conversion from the hexagonal crystal to the cubic one could be inhibited. C2ASH8 is a stable hexagonal crystal, which cannot induce the strength retrogression of the RW material. On 28 day, C3AH6 can be also detected in the RW material with SS mixing amount of 1%, it is because SS is consumed completely, which cannot react with all the hydrates of CAH10 and C2AH8, and the remaining CAH10 and C2AH8 are conversed to C3AH6. What's more, based on Fig. 5 and 6, the formation amount of C3AH6 in the RW material with SS of 1% is less than that in the RW material without SS, thus, the decrement of strength is less.
(7) |
According to the results of XRD and FT-IR, from 3 day to 14 day, the amounts of C–S–H (gel) and C2ASH8 in the RW materials containing SS of 4% are more than those in the RW material containing SS of 1%, which can explain the higher strength. Besides, there is no evidence of the formation of C3AH6 from 3 day to 28 day, indicating the silicate ions is so adequate that can consume CAH10 and C2AH8 fully. Therefore, the decrease in the long-term strength of the RW material can be inhibited effectively.
(1) The strength of the RW material could be enhanced by mixing with SS. And the more the SS content, the higher the strength. However, when the addition of SS less than 3%, the long-strength retrogression is existed in the RW material hydrated for 28 days. When SS mixing amount is above 3%, the strength retrogression of the RW material can be inhibited effectively.
(2) The compactness of the RW material is improved by the addition of SS. Compared with the RW material without SS, the RW material containing SS have a lower most probable pore diameter, due to the filling effect of C–S–H (gel) that is produced by the reaction between silicate ions and CH. And, whatever the amount of SS mixed, the compactness of the RW material increases over time, it can probably explain the strength enhancement during 3–14 day, but cannot explain the strength retrogression of the RW materials detected on 28 day.
(3) For the RW materials containing SS and hydrated for 0 to 14 day, there are more hexagonal hydrates and C–S–H (gel) and less AFt crystals, it is of benefit to the strength. However, the phase conversion of the hexagonal hydrates (CAH10 and C2AH8) to the cubic one (C3AH6) causes the strength retrogression of the RW materials with SS additions of 0 and 1%. Due to the reaction between silicate ions and CAH10 and C2AH8 to form C2ASH8, the content of C3AH6 in the RW material containing SS of 1% is less than that in the RW material without SS, that is the reason why the long-term strength decrement of the RW material containing SS of 1% is less than that of the RW material without SS. In addition, for the RW material with SS addition of 4%, the formation of C3AH6 is inhibited completely, thus, there is no long-term strength retrogression of the RW material.
This journal is © The Royal Society of Chemistry 2019 |