Roland Schierholz*a,
Daniel Krögera,
Henning Weinrichab,
Markus Gehringab,
Hermann Tempela,
Hans Kungla,
Joachim Mayercde and
Rüdiger-A. Eichelabc
aForschungszentrum Jülich GmbH, Institute of Energy and Climate Research, Fundamental Electrochemistry (IEK-9), Germany. E-mail: r.schierholz@fz-juelich.de
bInstitute of Physical Chemistry, Rheinisch Westfälische Technische Hochschule Aachen, Germany
cJülich Aachen Research Alliance: JARA-Energy, Germany
dForschungszentrum Jülich GmbH, Ernst Ruska-Centre (ER-C) for Microscopy and Spectroscopy with Electrons, Germany
eCentral Facility for Electron Microscopy, Rheinisch Westfälische Technische Hochschule Aachen, Germany
First published on 21st February 2019
Cathode structures derived from carbonized electrospun polyacrylonitrile (PAN) nanofibers are a current line of development for improvement of gas diffusion electrodes for metal–air batteries and fuel cells. Diameter, surface morphology, carbon structure and chemical composition of the carbon based fibers play a crucial role for the functionality of the resulting cathodes, especially with respect to oxygen adsorption properties, electrolyte wetting and electronic conductivity. These functionalities of the carbon fibers are strongly influenced by the carbonization process. Hitherto, fibers were mostly characterized by ex situ methods, which require great effort for statistical analysis in the case of microscopy. Here, we show the morphological and structural evolution of nanofibers during their carbonization at up to 1000 °C by in situ transmission electron microscopy (TEM). Changes in fiber diameter and surface morphology of individual nanofibers were observed at 250 °C, 600 °C, 800 °C and 1000 °C in imaging mode. The structural evolution was studied by concomitant high resolution TEM and electron diffraction. The results show with comparatively little effort shrinkage of the nanofiber diameter, roughening of the surface morphology and formation of turbostratic carbon with increasing carbonization temperature at identical locations.
After electrospinning the standard procedure to convert polymeric PAN-fibers into carbon fibers is oxidative stabilization, carbonization and graphitization.10 The first of these three steps is performed under air between 200 °C and 300 °C and the reactions involved are the cyclisation of nitrile and incorporation of oxygen as described by Goodhew et al.11 This step is important to avoid votalilization, maximize the carbon yield and avoid the formation of hollow core fibers in the subsequent carbonization step.10,12 The subsequent carbonization step is conducted under inert gas atmosphere up to temperatures of about 1500 °C. For higher temperatures, generally above 2500 °C, the term graphitization is used.10 Graphitization is usually performed for “high modulus” carbon fibers, used for reinforced plastics and not discussed in this manuscript, which focuses on carbonization below 1500 °C. The carbonization step involves losses of oxygen and nitrogen, still present after crosslinking. The corresponding evaporation processes start at temperatures just above the stabilization temperature of e.g. 400 °C.13 However, most changes were reported for temperatures between 700 °C and 1200 °C.12 Consequently changes in chemistry and structure of the fibers, but also in their dimensions and surface morphology result from the carbonization step in this temperature range.
A wide scope of analytical techniques such as X-ray Photoelectron Spectroscopy (XPS), X-Ray Diffractometry (XRD), Raman, infrared-spectroscopy, thermogravimetry (TGA) and differential thermoanalysis (DTA) has been applied for the characterization of structure, crosslinking/stabilization and carbonization behavior of PAN-derived carbon fibers.7,14–20 While most of these methods provide an overall view on the fiber materials, a technique of choice in order to obtain localized information – in particular on the fiber surfaces – is transmission electron microscopy (TEM).
Most TEM-studies were performed to study strength structure-relationship of carbon microfibers. In 1976 for example Bennett21 did an extensive three-dimensional analysis of PAN-derived carbon fibers heat treated at 1000 °C, 1500 °C and 2500 °C using various TEM techniques such as bright and dark field TEM, high resolution transmission electron microscopy (HRTEM) and quantitative electron diffraction analysis on transverse and longitudinal cross-sections. A more recent HRTEM investigation of copolymerized acrylonitrile/itaconic acid fibers drawn from a spinneret in a coagulation bath is presented by Bai et al.22 Here, amorphous and ordered structures were identified even without heat treatment. Furthermore, while highly oriented structures were detected in the longitudinal sections, the cross-sections showed onion like spherical ordering as well as crystallites.
Laffont et al. performed HRTEM, electron energy loss spectroscopy (EELS) and XRD on different types of commercial PAN-derived carbonized microfibers. They report coherent turbostratic graphite with a d-spacing larger than 3.43 Å.23 This is larger than the value of 3.35 Å published for graphite.24,25 Moreover, the size of the stacks firstly remains small with L10 ≤ 4 nm (parallel to the graphitic planes) and L002 ≤ 1.3 nm (perpendicular to the graphitic planes), but increases with processing temperature from 300 °C to 1000 °C.23 EELS analysis of the K-edges of carbon, nitrogen and oxygen shows that a carbon content of 99% is achieved for carbonization at 1000 °C, while only little amount of oxygen (0.5–1% from initially 1–4%) remains in the fibers.23 More dramatic is I the change of nitrogen content from initially 1–12% it drops to zero after 1000 °C, after 800 °C 1–3% are reported.23 In addition Laffont et al. also studied the σ + π plasmon in the low loss region and show that the σ-plasmon shifts to higher energies for materials processed at higher temperature and correlate this with lower resistivity.23 In a later work Laffont et al. used a combination of EELS and XPS to study the bonding situation especially of nitrogen.26 In this study, they report an increase of about +7 at% during stabilization in air at 250 °C and a loss of up to −15 at% during subsequent carbonization at up to 1000 °C in N2-atmosphere. Depending on the fiber treatment after spinning significant amounts of nitrogen [N]/[C] ≈ 0.1 and oxygen [O]/[C] ≈ 0.05 remain in the fiber. The chemical composition and bonding situation of nitrogen in carbon fibers were also studied in detail by other groups using XPS to distinguish different bonding types of nitrogen for application in batteries and fuel cells.2,14,19
The previously described results were mostly related to microfibers with diameters ranging from 5 to 12 μm. Musiol et al. compared PAN-derived nano and microfibers heat treated at 1000 °C, 2000 °C and 2800 °C, and reported higher massloss for nanofibers, 61% residual mass for carbon microfibers and 45% residual mass for carbon nanofibers after a heat treatment at 1000 °C.18 HRTEM and Raman spectroscopy showed graphitization for fibers treated above 2000 °C while the 1000 °C fibers still appear quite amorphous.18 For the temperature range from 1500 °C to 2800 °C a development from relatively smooth to rough and ridged morphology was reported by Kurban et al.27 In all reports temperature ranges differ and also a variety of different investigation techniques is applied. It is shown that the change of chemical composition; carbon structure and morphology of the fibers strongly depend on the carbonization process as well as the treatment applied in the previous steps.18,26,27
Common feature of most microscopy investigations is that the comparison of structural and morphological characteristics was performed based on ex situ experiments. Indeed, ex situ analyses are advantageous with respect to flexibility of the fibers processing conditions as they are not limited by the in situ experiment. However, comparisons of fibers subject to small process variations require that the effects of the process variation exceed the scattering in characteristics of individual fibers. Otherwise, large efforts by statistical analysis of many samples are required to provide significant data for establishing correlations between processing parameters and structural as well as microstructural characteristics. An approach to circumvent this is, to investigate the evolution of fiber characteristics on identical locations on individual fibers during processing with in situ microscopy methods. A first attempt was applied by Prilutsky et al. for the case of the carbonization of electrospun PAN nanofibers containing carbon nanotubes in 2010.28 However, in their study a heating stage, where the whole 3 mm grid is heated up, was used. Due to their larger heating volume such heating stages as a result feature slow response times, inaccurate temperatures, sample instabilities and strong thermal drift, thus limit the TEM image resolution. In this study we aim on studying the shrinkage of fiber diameter, surface morphology as well as structural changes on the same fibers in one single in situ TEM heating experiment at four subsequent temperature stages – 250 °C, after oxidative stabilization, 600 °C, 800 °C and 1000 °C on an in situ heating holder based on micromechanical systems (MEMS).29 In contrast to the before mentioned system this in situ holder allows high resolution TEM images and electron diffraction in accurate temperatures without instabilities, which will help to acquire a conclusive picture for the evolution of electrospun PAN nanofibers during carbonization.
Fig. 1 Heating program applied during experiment (black) and the measured diameters at different stages of the experiments for six selected nanofibers are plotted as a function of time (colored). |
For three fibers (1, 3 and 6) investigations were limited to low resolution size analysis, which is supposed to involve only minor influence of the electron beam. Three other fibers (2, 4 and 5) were subject to high resolution imaging and diffraction, which implies substantially higher dose for the high resolution and longer exposure to the beam during the alignment of the microscope for electron diffraction. The atmosphere during the in situ carbonization was imposed by the ultra-high vacuum (UHV) conditions required in the TEM.31 After every heating period the sample holder was cooled down to ambient temperature by switching off the heating.
Fig. 2 Overview images of fiber 6 at different stages during the in situ experiment (a) 250 °C, (b) 600 °C, (c) 800 °C and (d) 1000 °C. |
Fig. 3 Intermediate resolution images showing the development of fiber 5 morphology at temperature steps (a) 250 °C, (b) 600 °C, (c) 800 °C and (d) 1000 °C. |
Fig. 5 (a) [0−10] and (b) [1−10] electron diffraction pattern of single crystalline graphite. (c) Calculated azimuthal intensities for reflection up to 103 with |ghkl| ≤ 6.5 nm−1. |
The {102}-, {004}- and {103}-planes contribute to the second subring with ghkl in the range from 5.5 to 6.5 nm−1. Due to their multiplicity and orientation the {102}- and {103}-planes form a rather homogenously distributed intensity in the azimuthal range. The texture observed within the second subring arises mainly from 004, the second order reflection of the (002)-planes. In the proposed structure sketched in Fig. 6(a), close to the nanofiber surface most of the graphitic (002)-planes are parallel to the electron beam and in diffraction condition. However, the rotation around the c-axis remains a degree of freedom and therefore the relative intensity of 002 and 004 is expected to be higher, compared to h0l- and hkl-reflections, which are excited for graphitic regions in 〈100〉 and 〈1−10〉 zone axis orientations only, as depicted in Fig. 5(a) and (b).
Fig. 6 Schematic sketch of the nanofiber texture showing the preferential alignment of {002}-planes parallel to the nanofibers surface. (a) Shows conditions of HRTEM images recorded at the side of the nanofiber in Fig. 4(a)–(d). In (b) the condition for Electron Diffraction (ED) with a selected area Aperture (SA) positioned in the central part of the nanofiber, as applied for electron diffraction in Fig. 7, is shown. The rotation around the c-axis remains a degree of freedom within the graphitic planes. |
The observed variation of scattered intensities with the azimuth could be reproduced by calculations using a simple model. Starting with the [0−10] zone axis diffraction pattern as depicted in Fig. 5(a) the variety of c-axis orientation within the plane perpendicular to the electron beam is introduced by a Gaussian distribution with σ = 60° around the azimuthal positions of the reflections. Furthermore the relative intensities of h0l- and hkl-reflections are artificially decreased by a factor of 0.5 to represent relative intensities of the higher order reflections in respect to 002. The resulting intensity for reflections up to 103 (ghkl ≤ 6.5 nm−1) is plotted as a function of the azimuthal angle in Fig. 5(c). An azimuthal angle of 0° and 180° corresponds to scattering parallel to the fiber axis, 90°and 270° perpendicular to the fiber axis. The thick dashed lines represent I100 + I101 (red) and I102 + I004 + I103 (blue), which in first approximation can be attributed to the inner and outer subring of the former diffuse second ring in the FFTs in Fig. 4(b–d). Furthermore, the graph represents the higher intensity parallel to the fiber axis for the inner subring (red) and the higher intensity of the second subring (blue) perpendicular to the fiber axis.
Enhanced ordering in the graphitic structure under the influence of high temperatures is also visible at fracture surfaces at the tip of the nanofiber pieces (Fig. 4(e–h)). In contrast to the turbostratic structures formed on the lateral surfaces no preferential orientation of the turbostratic areas can be recognized in the real space image. Confirming this observation, the FFTs shown in the insets of Fig. 4(e–h) show rings with homogeneously distributed intensity in the azimuthal range as expected for randomly oriented crystallites. With increasing temperature these rings just get sharper and more defined. The interpretation of these observations is sketched in Fig. 6. As in the central part of the nanofiber the distance to the surface is comparable in all directions, so the ordered regions in this part of the nanofiber have arbitrary orientations among each other. Thus we conclude that ordering of carbon atoms in a turbostratic form applies also to the inner parts of the nanofiber. The 002-texture on the other hand is predominantly formed close to the nanofiber surface.
At 250 °C, three diffuse rings can be recognized in the diffraction pattern (Fig. 7(d)). At 600 °C (Fig. 7(e)), mainly the first, the 002-ring, becomes more defined and already starts to exhibit higher intensity for scattering vectors perpendicular to the fiber axis. For the second ring the intensity increase at low scattering vectors ≈ 4.6 nm−1 becomes sharper while the decay to larger scattering vectors stays rather diffuse. At 800 °C (Fig. 7(f)), the texture in the 002-ring becomes more pronounced and the former second diffuse ring splits into two distinguishable rings, of which the first one at lower scattering vectors is of higher intensity.The evolution of the diffraction patterns as described above can be followed in the background subtracted radial intensity, which was extracted from the diffraction patterns plotted in Fig. 7(g–i). An exponential background in the form of eqn (1)
a1e−b1(μ1−x) + a2e−b2(μ2−x) + d | (1) |
Within the diffraction patterns, only the first ring originates from a single reflection, which is 002. The position of its maximum at 800 °C is found at ≈2.84 nm−1 corresponding to a d002-spacing of 352 pm. The second ring already contains five reflections, 100, 101, 102, 004 and 103. The sharp increase of intensity at low scattering vectors can be attributed to the rather closely packed 100 (4.694 nm−1 Irel ≈ 3%) and 101 (4.925 nm−1 Irel ≈ 18%). Among the five reflections contributing the second ring 101 is by far the most intense reflection. The diffuse decay to larger scattering vectors can be attributed to more broadly distributed 102 (5.560 nm−1 Irel = 3%), 004 (5.961 nm−1 Irel = 7%) and 103 (6.482 nm−1 Irel = 5%) reflections. At 800 °C, two separate rings become distinguishable in the formerly second ring, which can be attributed to these previously described two groups of reflections. We attribute the first subring to 001 and 101, the second subring to 102, 004 and 103 reflections. As the first subring is dominated by 101, it shows higher intensity parallel to the fiber axis. For the second subring the highest intensity is observed for scattering perpendicular to the fiber axis, which can only arise from 004. Both observations can be explained by the calculated azimuthal intensity distribution shown in Fig. 6(c). The same texture also influences the relative intensity of the reflections under the third main ring in the range from ≈7.5 nm−1 to ≈10 nm−1. In this range 110 (5.4%) and 112 (8.7%) are the most intense reflections and show higher intensity parallel to the fiber axis.
The texture evolution can be followed by comparing the background subtracted radial intensities parallel and perpendicular to the fiber axis. At 250 °C, no significant difference between scattering parallel and perpendicular (b) to the fiber axis is noticed. At 600 °C, the 002-intensity is already much stronger perpendicular to the fiber and lower parallel to the fiber axis. Perpendicular to the fiber axis for the second ring a hump between 5.5 and 6 nm−1 can be recognized next to the reduced main peak, which is formed by the 101 reflection (4.925 nm−1 Irel ≈ 18%) with little contributions of 100 (4.694 nm−1 Irel ≈ 3%). This hump can be explained with the 004 peak (5.952 nm−1), which is the second order reflection of 002. Parallel to the fiber axis 004 is less intense and the main peak is dominated by 101 and shows only long decay towards larger scattering vectors. At 800 °C, this behavior becomes even more pronounced. Nevertheless, the texture effect in the two subrings of the second ring in the diffraction patterns in Fig. 7(e) and (f) is much weaker than in the FFTs of the HRTEM micrographs recorded at the side surface of fiber 5 in Fig. 4(b–d).
During the last heating step up to 1000 °C, the nanofiber selected for diffraction moved on the heating chip, so the orientation of the fiber and the position of the selected area aperture are not identical to the previous measurements at the other temperatures. Nevertheless, a diffraction pattern was recorded and is displayed in Fig. 8 together with the corresponding micrograph as well as with the radial intensity extracted parallel and perpendicular to the fiber axis. According to the different fiber orientation, the angular ranges for extracting the radial intensities parallel and perpendicular to the fiber axis changed to 175–215° (parallel) and 265–305° (perpendicular). The texture effects at 1000 °C are more pronounced compared to the results at lower temperatures, with almost equal intensity of 002 and 100 + 101 parallel to the fiber axis. The presence of texture in diffraction arising from a volume close to the center of the fiber means the texture is also present inside the fiber. The observation of diffraction rings up to 10 nm−1 correlates with an extended graphitic order. This is supported by Raman spectra measured ex situ on fiber mats carbonized for 10 h in argon atmosphere at the same temperatures shown in Fig. S3.† The spectra are scaled to the D-band maximum at around 1350 cm−1. An increase of G-band intensity around 1580 cm−1 with increasing carbonization temperature is clearly visible.
By intermediate TEM magnification micrographs, we observed a marked increase of the nanofiber roughness, especially in the first heating step to 600 °C. The surface roughening was accompanied by diffraction contrast arising inside the fibers. Roughening of carbon nanofibers derived from electrospun PAN upon graphitization at higher temperatures of 1500 and 2800 °C was also reported by Kurban et al.27 Bennett used diffraction contrast in dark-field TEM to image regions of turbostratic graphite in carbon microfibers treated at temperatures.21 In our study, we observe regions with sizes around 5 nm after 600 °C and up to 10 nm after 800 °C or even up to15 nm at 1000 °C. These sizes agree with our HRTEM micrographs, where we estimate the size of ordered regions within the graphitic plane (L10 or La) and perpendicular to them (L002 or Lc) of few nm at 600 °C, up to 5 nm at 800 °C and up to 10 nm at 1000 °C. So the interpretation as diffraction contrast arising from turbostratic carbon is valid. A slightly higher measure in diffraction contrast is not surprising as the field of view and the statistics are better the image resolution poorer. In our case the estimated sizes in and out of plane are comparable. Laffont et al. retrieved L10 ≈ 3–4 nm by Warren Bodenstein formula and L002 ≈ 1 nm retrieved from the Scherrer equation, both from XRD results.23,33 Kim et al. achieves similar results for Lc from XRD via the Scherrer equation.34 In their work the values for L10 (or La) extracted from Raman spectra via the Knight and White equation are also larger than the values of L002.34,35 Deviations of sizes measured with different methods can be expected. In addition results are sensitive to experimental conditions and the initial fibers used.
In agreement with literature we observed a preferential alignment of the graphitic planes with the fiber axis.18,21,22,27,34 This texture is confirmed by the FFTs of the HRTEM images as well as the electron diffraction patterns. Comparing our HRTEM micrographs to others the graphitic regions in our experiment appear more disordered with planes more bend and also the borders of the ordered regions are less defined.18,21,22,27,34 Most similarity is found with the micrographs published by Kim et al. However clearly in our micrographs a higher number of planes stacked corresponding to higher Lc is visible.20 The curvature of graphitic planes observed in HRTEM is well reflected by the rather broad peaks in the azimuthal distribution within the diffraction rings in the FFTs and the electron diffraction patterns. We achieved good agreement of the experimentally observed azimuthal intensity distribution with calculated intensities based on a simple model, which correlates to a variation in orientation of the graphitic (002)-planes. A different degree of texture for HRTEM-micrographs recorded at the fiber surface, the broken tip of the nanofiber and electron diffraction was observed. This can be explained with the volume probed in each experiment. In the HRTEM micrographs of the fiber surface in Fig. 4(a–d) only the structure of the surface up to a depth of ≈30 nm is probed. With the texture proposed in Fig. 5(a), similar to that suggested by Bennet for microfibers, most of the (002)-planes are parallel to the electron beam in this region of the fiber resulting in enhancement of 002-reflection compared to the averaged structure.11 In the electron diffraction experiment on the other hand, the selected area aperture is positioned more central to the fiber axis (Fig. 5(b) and 7(a–c)) so diffraction arises from the central volume of the fiber plus the upper and lower surface. In this part of the fiber (002)-planes are expected in perpendicular orientation to the electron beam and therefore not in diffraction condition. The aperture with a diameter of ≈170 μm in the intermediate image plane cuts of regions close to the surface which contribute to the HRTEM-micrographs taken at the fiber surface. Nevertheless texture effects are observed, underlining that, even with some distance to the nanofiber surface, the texture still is present. However, the HRTEM-micrographs recorded at the broken tip of a nanofiber don't show texture. Within the region chosen there, the turbostratic carbon is randomly oriented. We propose to apply both HRTEM and diffraction as these two techniques are complementary in respect to the volume probed. While for the analysis of nanofibers designed for mechanical applications the knowledge about the structures in the fiber cores is crucial, properties of the surfaces and surface near regions are the most relevant for the application of nanofibers in electrodes for metal–air batteries, fuel cells or electrocatalysis.
Quantitative analysis of the diffraction data showed that the 002 peak stabilizes around 2.84 nm−1 at 800 °C and 1000 °C corresponding to a d002-spacing of 352 pm compared to 335 pm for graphite.25 Laffont et al. and Kim et al. reported during stabilization like our fiber mat, after 1000 °C heat treatment part of the nitrogen remains in the fiber.20,26 However, in the case of an in situ TEM experiment an influence of UHV compared to inert gas atmosphere in an ex situ experiment on d002-values of 349 pm and 357 pm respectively for PAN derived carbon fibers.23,34 Our result is comparable to both of them. Kim et al. attribute the stacking distance to the presence of quaternary nitrogen.20 Laffont et al. showed that in fiber set 2, which was allowed to shrink the nitrogen content is possible. If the microscope is equipped with a spectrometer, the chemical composition can be tracked by EELS or EDX during the in situ experiment.
As shown above the techniques available in a TEM allow a broad spectrum of analysis to study the carbonization of PAN-derived nanofiber during an in situ experiment. Results are at least comparable to ex situ experiments. However, it has to be kept in mind that a complete reproduction of ex situ experiments inside the TEM is not possible as parameters such as heating rate and atmosphere affect the final properties of the nanofibers.34,36 Combined in situ heating experiments under gas flow, which are possible nowadays, could help to circumvent this issue. During the first 250 °C heating step some influence of the electron beam was evidenced from the substantial difference in fiber diameter shrinkage, depending on the exposure of the nanofiber to the electron beam. The latter might be attributed to the interaction of the electron beam with residual gases in the microscope and the applied heating of the sample.37–39 The fibers with higher exposure to the electron beam under UHV conditions at 250 °C show faster shrinkage. Also an influence on the surface roughness is possible. This could be controlled by a comparison with additional ex situ experiments on identical locations. In any case, the beam exposure should be kept to a minimum, which we did for the rest of the fibers. With respect to the main subject of research – the formation of graphitic structures in the fibers depending on carbonization temperature – this confinement does not preclude the in situ method for these objectives.
With the combination of TEM at low, intermediate and high magnification and electron diffraction we were able to follow the shrinkage of fiber diameter and the development of the surface morphology as well as the carbon structure during the in situ experiment. In combination with complementary ex situ experiments, the in situ experiments can contribute to an overall picture of the carbonization process for polymer-derived carbon nanofibers. Thus, the in situ carbonization TEM technique provides a promising approach which is currently just at the beginning of its development.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c8ra10491c |