Ahmed A. Aboud*a,
Mohamed Shabana and
Neerish Revaprasadub
aDepartment of Physics, Faculty of Science, Beni-Suef University, Beni-Suef, 62514, Egypt. E-mail: ahmed.mostafa@science.bsu.edu.eg
bDepartment of Chemistry, University of Zululand, Private Bag X1001, Kwa-Dlangezwa, 3886, South Africa
First published on 7th March 2019
In the present study, the effects of metallic doping on the photoelectron\chemical properties of zinc oxide thin films have been studied. All films have been deposited using the spray pyrolysis technique at a constant doping level of 3 wt% whereby Cu, Ni, and Pb were used as dopants. The structure of all films was studied by X-ray diffraction which showed the grain size of all doped films to be 50 nm. The energy band gap of all films was estimated using optical transmission spectroscopy. The Ni, Cu, and Pb-doped ZnO photoelectrodes were applied for the photoelectrochemical (PEC) H2 generation from H2O. Pb doping leads to the highest photocurrent of the ZnO photoelectrodes. The current density–potential characteristics were measured under white light and monochromatic illumination. The stability of the electrode was quantified as a function of the number of H2 production runs and exposure time. Finally, the incident photon-to-current conversion efficiency, IPCE, and applied bias photon-to-current efficiency, ABPE, were calculated. The optimum IPCE at 390 nm was ∼30% whereas the ABPE was 0.636 at 0.5 V.
ZnO is a wide bandgap n-type semiconductor with a band gap value of 3.2 eV with an anisotropic crystal structure.13,14 It has been extensively studied and its properties well reported.4,15,16 Also, non-toxicity, abundance in nature, low-cost and easy synthesis, massive production, and high thermal stability are advantageous properties of ZnO.17,18 Moreover, the morphologies of ZnO can be tuned to produce a large variety of superstructures with different morphologies and orientations due to it's hexagonal (wurtzite) crystal.13,19,20
The PEC water splitting is a complex thermodynamic process that required the participation of two water molecules in two steps to split the atoms in H2O. The products are separated based on the reduction half-reaction [2H+ + 2e− → (Ered = 0.00 V/RHE)] and oxidation half-reaction [2H2O + 4h+ → O2 + 4H+ (Eoxi = −1.23 V/RHE)]. The overall PEC reaction can be represented as 2H2O → 2H2 + O2 (ΔE = −1.23 V/RHE).21 Since H2O oxidation is the rate-limiting reaction in the overall PEC water splitting, the design of an efficient photoanode is an important barrier to overcome to perform this reaction.22
For efficient PEC water splitting, ZnO is a prominent semiconductor owing to its low cost and high catalytic efficiency. ZnO nanostructures have shown interesting results in PEC water splitting because of their outstanding electrochemical properties.23 Rokade et al.24 designed 1D ZnO nanorods and nanotubes (NTs) by the electrodeposition method, the nanotube structure showed enhanced hydrogen PEC current density of 0.67 A cm−2 at 0.5 V over the nanorod morphology.
In addition, M. Liu et al.25 investigated the water splitting and chemical stability of ZnO/titania core/shell nanowire photoanodes, which showed 25% higher PEC water splitting activity than the as-deposited ZnO. Zhang et al. showed that the design of high-quality ZnO films with limited deep trap states and thickness greater than the light absorption depth and space charge region width provided a long photocarrier lifetime with a high quantum efficiency (>80%).26
Also, Hoang et al.27 fabricated an arrayed structure of CdS-sensitized ZnO nanorods on ITO substrates for PEC hydrogen generation. They got maximum photoconversion efficiency (2.7%) under solar irradiation of 100 mW cm−2 for PEC hydrogen generation using the electrode grown for 3 h. The maximum hydrogen rate was 22 mL cm−2 after 1 h exposure. Moreover, Bouhjar et al.21,28 showed that the PEC efficiency of the hydrothermally grown α-Fe2O3/ZnO heterojunction is higher than that of FTO/α-Fe2O3 and FTO/ZnO. Furthermore, Kim et al.29 introduced complex co-sensitized ZnO/WOx heterostructures for efficient visible light absorption and PEC hydrogen production.
The CdSe/CdS co-sensitized ZnO/WOx showed effective charge transport and produced a high PEC current density of 11 mA cm−2 at 0.5 V. Desai et al.30 recently discussed different modern approaches for producing different morphologies of ZnO superstructures and highlighted their role in improving PEC performance towards the efficient production of hydrogen.
Appavoo et al.31 used in situ ultrafast spectroscopy to quantify the recombination processes (bulk and surface) in nanostructured photocatalysts for PEC water splitting and showed how these recombination processes limit the overall efficiency. Moreover, Cen et al.32 showed that different in situ spectroscopic and microscopic methods can be combined to develop mechanistic information about all features of PEC-WS.
The application of ZnO and ZnO-based structures in solar water splitting is still limited due to its high band gap energy, poor stability in aqueous media, insufficient photo-conversion efficiency, charge transfer resistance, or complicated architecture.33–36 Therefore, it is meaningful to address a low-cost and straightforward strategy to introduce different metal doping to 1D ZnO nanostructured films. The metal-doped ZnO with high charge carrier density (electrical conductivity) and enhanced light absorption is introduced to improve PEC performance. Also, in order to utilize such materials in PEC applications, the band gap value has to be reduced. N-doping has been used to shrink the ZnO band gap.15,16,37 Sundhakar et al.16 studied the effect of Al and N co-doping on the PEC activity of r.f. magnetron sputtered ZnO thin films on FTO glass without addressing stability and evaluation of PEC performance. Moreover, compared with other methods such as r.f. magnetron sputtering, chemical vapour deposition (CVD), and plasma chemical vapour deposition (PCVD). The spray pyrolysis technique has been known to be highly cost-effective and adaptable for the deposition of doped ZnO.
In this paper, we report the deposition of pure, Cu, Ni and Pb-doped zinc oxide thin films by the spray pyrolysis technique. All films have been obtained using the same deposition parameters except the type of the dopant. The structural, optical, and PEC properties are studied and discussed. Finally, electrode stability and PEC performance are evaluated under monochromatic and white light illumination to elucidate the effect of doping.
Ni, Cu, and Pb-doped ZnO electrodes were used as working electrodes for photocatalytic hydrogen generation water splitting experiments. The PEC behaviour was measured under illumination of 500 W Mercury-Xenon Light Source (Newport, 66926-500HX-R07) provided with a series of linear optical filters in 0.3 M (100 mL) Na2S2O3 solution at room temperature (25 °C) with a sweep rate of 1 mV s−1. The schematic diagram of the used PEC cell is shown in Fig. 5. The area of the used electrode is 1 cm2, the counter electrode being Pt-electrode, and the reference electrode, Ag/AgCl. The PEC current density–potential (Jph–E) and the current density–time (Jph–t) behaviours were recorded with a Keithley measurement source unit using LabTracer software (2400 Source Meter, A Tektronix Company).
Film | a (Å) | c (Å) | GS (nm) | Strain | Stress | u | L | Thickness (nm) | Band gap (eV) |
---|---|---|---|---|---|---|---|---|---|
Pure | 3.259596 | 5.21282 | 65 | 0.001117726 | −260430190.1 | 0.380335 | 1.885729 | 753 | 3.2 |
Cu | 3.250922 | 5.2028 | 50 | −0.00080661 | 187939312.5 | 0.380142 | 1.880744 | 535 | 3.2 |
Ni | 3.257866 | 5.21392 | 50 | 0.00132898 | −309652391 | 0.380142 | 1.884745 | 482 | 3.2 |
Pb | 3.25681 | 5.21608 | 50 | 0.001743806 | −406306894.6 | 0.37995 | 1.884148 | 600 | 3.3 |
In all films, no other crystalline phases could be detected confirming the singularity of the hexagonal ZnO phase and the successful doping process. As observed, the main peak intensity decreases as a function of the dopant type. This could be attributed to the close ionic radii values between Zn and all dopants except Pb (Pb4+ = 0.78 Å (ref. 38) and Ni+2 = 0.69 Å,39 Cu+2 = 0.73 Å, Cu+ = 0.77 Å,40 Zn+2 = 0.74 Å (ref. 41)).
The grain size was calculated depending on the full width at half maximum (FWHM). The FWHM was found to increase upon doping. Such an increase in the FWHM value reflects the increase in the imperfections due to the increase in the internal microstrain within the film accompanied with a reduction in the grain size value. The grain size was estimated according to Scherrer's equation:42-
The influence of Cu-doping on the crystallization quality of ZnO thin films is attributed to the radius of Cu2+ (0.73 Å) bring less than that of Zn2+ (0.74 Å). When Cu2+ was incorporated in the ZnO lattice, the structure around Cu is deformed in small areas and the lattice constants decreases, see Table 1. Wang et al.44 observed the reduction of the (002) peak intensity for Cu-doped ZnO thin films prepared using the sputtering technique. This reduction in the peak intensity has been attributed to Cu-atoms which exist as interstitial instead of substitution positions where Cu+ and Cu2+ can be detected by XPS.
Doping of ZnO films with Ni+2 ions does not have appreciable effect on the crystal structure of the films as recorded by Reddy et al.47 for films deposited using the spray pyrolysis technique. But in the work of Patil et al.48 the grain size was found to increase first when the Ni content is lower than 1.5%. After this percentage the grain size was found to decrease with decrease in intensity of the (002) diffraction peak. Abdel-Wahab et al.49 recorded a crystallinity degradation of ZnO thin films upon Ni-doping. At Ni 7 wt% concentration, the (002) disappears. From the variations and disappearing of the peaks, it can be assumed that the doping of Ni modifies the film growth. Similar results can be observed by Nunes et al.50 and El Manouni et al.51 Also the degradation of the grain size upon Ni doping has been reported previously by Kim et al.52 İskenderoğlu et al.46 studied the impact of Ni-doping on the properties of ZnO thin films prepared by the spray pyrolysis technique. They found that the grain size decreased upon doping up to Ni-concentration of 6%. Thereafter the grain size starts to grow again.
Turgut et al.53 studied the effect of Pb doping on the properties of ZnO thin films deposited using sol–gel technique. They found that the (002) peak intensity decreases with Pb incorporation at high level where the films shows an amorphous nature at doping level 30 wt%.
Generally, the reduction in the grain size can be attributed in the frame of Zener pining effect with dopant acting as obstacle to inhibit grain growth. The limiting grain size, D, is generally given as a function of the mean radius of the pinning particles, R, and their volume of fraction, fv;45
The strain (ε) and stress (σ) in the film, along the c-axis, were estimated using the following equations:54-
Zhong et al.39 studied the effect of Ni-doping on the properties of ZnO thin films where a compressive stress is found due to the substitution of Zn2+ (0.74 nm) with Ni2+ (0.69 nm). This result is in contradiction to ours where a tensile stress is found. That may suggest an interstitial doping of a small amount of Ni-ions in the network of ZnO.
The obtained values indicate the presence of a compressive strain in the case of Cu-doping and tensile strain is observed in the case of pure, Ni and Pb doped films. The lattice parameters of all films have been estimated from the equation:54-
The variation in the lattice parameters values are listed in Table 1, a and c. This behavior could be attributed to the ionic radii value as mentioned above.
The Zn–O bond length (L) was also estimated using the following equations:54-
Fig. 2 shows the SEM images of the surfaces of pure and doped ZnO thin films. The average particle size has been calculated for all films using the cross section method. The average size was found to be 65.8, 102.75, 78.2 and 118 nm for pure, Cu, Ni and Pb doped ZnO thin films respectively. Comparing these results with the XRD values result we get a perfect match in the case of pure ZnO films. In the doped film cases higher sizes are measured from the SEM technique than XRD. The shift in the case of Ni-doped films is small but approximately doubles in size in the case of Cu and Pb doped films. That could be attributed to an agglomeration process take place during film formation. Circular grains are observed in pure and Cu-doped thin films. Different particles morphologies are noticed in the cases of Ni and Pb doped films. That could be attributed to the change in the growth mode with increasing the film thickness for the doped ZnO film. The EDX analysis shows the existence of the doped elements in all films. The atomic ratios of Cu, Ni and Pb percentage to Zn was found to be 10.95, 2.2 and 5.6% respectively.
Fig. 3 shows the transmission spectra of all films in the spectral range of 200–1100 nm wavelength. All films show interference fringes which facilitate the thickness extraction from the transmission spectra using Swanepoel's method. As listed in Table 1 the thickness shows random variation against the type of doping. Generally it decreased upon doping. The Pb-doped film is thicker than Cu-doped films which in turn is thicker than the Ni-doped films. Such variation in the film thickness could be attributed to the reduction in the c-axis growth of all doped films with respect to the pure zinc oxide film. Also doping may cause a reduction in the reaction rate which slows down the film formation on the surface of the substrate. As an example of that, the bond length of Pb–O (2.49 Å (ref. 55)) is larger than Zn–O (1.97 Å (ref. 56)) bond length. This reflects that the energy of the Pb–O bond is lower than the Zn–O bond. This makes it easier for the oxygen attached to the Pb atom to escape to the film than the oxygen attached to Zn-ions. That will not help to bring more materials in the film bulk and help to decrease the film thickness. Also the generated strain in all films, compressive or tensile, leads to an increase in the strain energy which limits the dopant solubility in the host ZnO.57 The thickness of ZnO thin films shows a random variation upon doping as recorded by Bouznit et al.58
A general reduction in the transmission level can be observed upon ZnO doping. The average transmission of all film was found to decrease from 83.7, 78.61, 81.65 and 77.2 for pure and Cu, Pb and Ni doped ZnO films in the spectral range 500–1100 nm. The inset at the lower corner in Fig. 2 showed an enlarged part of the high absorption region in the transmission spectra in the range of 360–580 nm. Except for the Pb doped film, there is no shift in the cut off wavelength in transmission.
The thickness of all films was determined using the Prava program.59 The thickness values are listed in Table 1. As recorded, the thicknesses of all doped films were lower than the pure ZnO film.
Fig. 3 shows the plots of (αhν)2 against hν in order to estimate the band gap values of the deposited films. The band gap energy values Eg was estimated using the equation of Tauc's;60
(αhν)2 = A(hν − Eg) |
In the case of Cu doping, the band gap was fund to be constant. That may be attributed to the low doping level which is not enough, in this case, to produce a notable shift in the band gap value of ZnO thin films even with the change in the degree of crystallinity which recorded. In the work of Jongnavakit et al.45 and Sreedhar et al.61 the band gap was found to increase with increasing Cu doping. This increase in the band gap has been attributed to the strong mismatch in the electronegativity of Cu and Zn atoms in ZnO. This effect may be compensated by the reduction in the degree of crystallinity found in our work. Reduction in crystallinity may introduce energy states in the band gap region which cause a reduction in the band gap value. The same result was recorded in ZnO thin films upon Ni doping in other work.
Ni-doping is known to decrease the band gap of ZnO thin films.46,49 The decrease in the band gap has been attributed to the strong sp–d exchange interaction between the band electrons and the localized ‘d’ electrons of the Ni ions substituted in the Zn sites in 10 at% Ni doping level.46,62,63
In our work the band gap was found to be constant in the case of Cu and Ni doping films while increasing in the Pb doped film. The constant band gap in the Cu and Ni doped films could be attributed to the low concentration of dopants which make no shift in the band gap value.63
On the other hand the optical band gap increases in the Pb doped films. Since the ionic radii of Pb2+ (1.29 Å) and Pb4+ (0.78 Å) are larger than the ionic radii of Zn2+ (0.74 Å), Zn2+ can be replaced by Pb4+ more easily than Pb2+ due to its close ionic radii. If Zn2+ ions are replaced by Pb4+ ions in the ZnO structure, Pb4+ ions will introduce two electrons into the ZnO, so it is expected to increase the charge carrier concentration and increase the oxygen content in the film. Such increase in the charge carrier concentration is the reason for the increase in the band gap upon Pb doping according to Moss–Burstein effect. Such increase in the band gap value upon Pb doping in ZnO thin films was recorded by Turgut et al.53
Fig. 5 shows the PEC behaviors of the Pb-doped ZnO electrode under white light illumination. As shown in Fig. 5(a), the power density was varied from 50 to 100 mW cm−2. As the power density increased, the current density is linearly increased with a rate of 61.2 mA W−1, Fig. 5(b). Upon exposure to light, the large surface area of the electrode will produce a high density of electron–hole pairs, which will motivate the splitting of H2O molecules under the effect of light to carry out the PEC reaction. From Fig. 5(a), the Pb-doped ZnO electrode is affected by the light and works as a photoanode. The current density values for an electrode at dark and light is 0.4 and 8 mA cm−2 at 1 V, respectively. This indicates an efficient electrochemical water splitting utilizing the Pb-doped ZnO electrode. The stability of the Pb-doped ZnO electrode for H2 generation was investigated as a function in the number of measurement runs and as a function of the illumination time. As shown in Fig. 5(a) and its inset, the current density-potential measurements were carried out for six successive runs at power density 100 mW cm−2. As the number of runs increased, the current density decreased from 8 to 7.22 mA cm−2 at 1 V. Then after 6 runs, the degradation rate of the photocurrent density for Pb-doped ZnO electrode was approximately 10%. Also, the stability of the Pb-doped ZnO electrode for H2 generation was investigated under white light illumination for a prolonged time as shown in Fig. 5(c). During this measurement, a small bias voltage of 0.6 V was applied between the photoanode and the counter electrode to overcome any external losses of the measuring system. The current density decreased sharply in the first period (130 s) from 8.88 to 0.29 mA cm−2, then almost constant till 1800 s, in which the accumulated ionic charges are increased, suggesting a longer lifetime of the suggested electrode to work in the PEC-water splitting experiment. It was reported that the high density of surface states might lead to a significant pinning of the Fermi level that can facilitate the participation of these defect states in the surface oxidation process, leading to a significant degradation of the photoanode.64,65
Fig. 6(a) shows the variation of photocurrent density with the potential from 0 to 0.65 V under the illumination of monochromatic light on Pb-doped ZnO electrode. The optical filters of different wavelengths from 390 to 636 nm are used to control the illumination at 25 °C. From the figure, the current density increases with increasing the incident wavelength from 390 to 460 nm; then it decreases as the wavelength increases from 460 to 636 nm. The illumination with light of wavelength 460 nm showed the highest response, however the longer wavelength, 636 nm, showed the lowest response.
Fig. 6 Photocurrent density-potential behavior for (a) Ni, (b) Cu, and (c) Pb-doped ZnO electrodes under dark and white light illumination at 298 K. |
This behaviour matches with the optical UV-visible analyses data as shown in Fig. 2. The behaviour of the photoanode can be tentatively attributed to the enhanced solar absorption that can cover a large portion of the solar spectrum. The photostability of the Pb-doped ZnO photoanode was also investigated during PEC reaction under different monochromatic light illumination. Fig. 6(b) shows the variation of photocurrent density with the illumination time at 0.6 V under the illumination of monochromatic light of different wavelengths. It can be seen that, during PEC water splitting reaction, the photocurrent density increased for the first 900 s of irradiation before becoming stable. This increased current density can be attributed to the modification of the surface of the electrode; a similar phenomenon was previously reported for the different types of electrodes.66–68
The enhanced solar absorption of the Pb-doped ZnO photoanode was further confirmed by measuring the incident photon-to-current conversion efficiency (IPCE) under monochromatic illumination conditions. Such analytical measurements can also give meaningful insight into the contribution of Pb-doped ZnO electrode in the conversion of the incident photons into charge carriers. The IPCE was determined at an applied potential of 0.5 V from eqn (1) and shown in Fig. 7(a):68,69
(1) |
To fully evaluate the PEC-water splitting performance of the Pb-doped ZnO photoanode, we further measured the applied bias photon-to-current efficiency (ABPE), which can allow diagnostic measurements represent the development of the electrode performance as a function of the applied potential. The measured ABPE values for the Pb-doped ZnO photoanode was calculated by using eqn (2): 68,70
(2) |
Fig. 8 (a) Photocurrent density-potential and (b) photocurrent density–time characteristics under different monochromatic light illumination at 298 K. |
This journal is © The Royal Society of Chemistry 2019 |