The thermal conductivities of GeTe/Bi2Te3 superlattice-like materials are calculated based on density functional perturbation theory (DFPT) and measured using a 3ω method. The calculated results show that the lattice thermal conductivity or thermal diffusivity of GeTe/Bi2Te3 superlattice-like materials significantly decrease due to the effects of interfaces and Bi atoms in Bi2Te3. Our measured results are in line with the theoretical calculations, and reach an extremely low thermal conductivity at 0.162 W mK−1 compared with published work on Ge–Sb(Bi)–Te, indicating the effectiveness of modulating the thermal properties of phase change materials by using Bi-based GeTe/Bi2Te3 superlattice-like materials. Our findings give a calculation method to modify the thermal characteristics of superlattice-like materials and confirm Bi-based GeTe/Bi2Te3 superlattice-like materials as promising candidates for phase change materials with lower thermal conductivity.
Bi2Te3 has rhombohedral crystal structure belonging to the space group R3m with five atoms in one unit cell, the lattice parameters of the five-layer hexagonal unit cell built up by three formula units are a = b = 4.384 Å, c = 30.497 Å, and α = β = 90°, γ = 120°.11 For GeTe, a distorted rocksalt structure with a = b = c = 5.996 Å and α = β = γ = 90°, belonging to space group R3m.12 The crystal structures of the GTBT (GeTe/Bi2Te3) superlattices were constructed from the <001> direction of trigonal Bi2Te3 and the <111> direction of cubic GeTe, thus superlattices exhibit high quality interfaces due to the good lattice parameter match. We consider that the interfacial state and the strength of the Bi atoms' influence on interfaces may have effect on the thermal conductivity. In order to support the conjecture, we choose four common superlattice structures with different number of interfaces or different distance between Bi atoms and interfaces. Table 1 lists the lattice constants of the four GTBT superlattice structures with the Petrov,13 inverted Petrov,14 Kooi, and Ferro-GeTe15 phase using PBE. Additionally, the features of superlattice structures, including the number of the long distance Te–Te interfaces (Ni) and the number of Bi atoms near to the interfaces (Nn), are also shown. Meanwhile, GTST (GeTe/Sb2Te3) as common superlattice materials are also listed to providing comprehensive analysis of the thermal property change trend with GTBT superlattices in same structures, and the lattice parameters of the five-layer hexagonal unit cell in Sb2Te3 are a = b = 4.264 Å, c = 30.458 Å, and α = β = 90°, γ = 120°. For both GTBT and GTST superlattice structures, the lattice parameter a = b, and α = 90°, β = 90°, γ = 120°.
Inverted Petrov | Petrov | |||||||
---|---|---|---|---|---|---|---|---|
a (b) (Å) | c (Å) | Ni | Nn | a (b) (Å) | c (Å) | Ni | Nn | |
GTST | 4.205 | 19.405 | 2 | 2 | 4.266 | 17.982 | 1 | 0 |
GTBT | 4.269 | 19.445 | 4.327 | 18.143 |
Ferro-GeTe | Kooi | |||||||
---|---|---|---|---|---|---|---|---|
a (b) (Å) | c (Å) | Ni | Nn | a (b) (Å) | c (Å) | Ni | Nn | |
GTST | 4.283 | 17.677 | 1 | 1 | 4.293 | 17.632 | — | — |
GTBT | 4.341 | 17.893 | 4.353 | 17.934 |
The crystal structures of GTBT superlattice are illustrated in Fig. 1, and the corresponding phonon dispersion curves along the out-of-plane direction (Γ–Z direction) are shown in the right column. The PHONOPY code16 was performed to calculate the phonon frequencies through a supercell method. In calculating the force constants in real space we use density functional perturbation theory (DFPT) together with 72 atoms 2 × 2 × 2 supercells, the phonon band structure and density of states are generated from the force constants.
For further studying the source of the significant small group velocity in GTBT superlattice structures, we calculated the phonon dispersion curves and the PhDOS of superlattice structures. The result of superlattice structures with inverted Petrov phase were chosen as an example to discussed. As shown in Fig. 2, we plot the calculated phonon dispersion curves along the Γ–A–K–Γ–M–K direction for GTBT superlattices with inverted Petrov phase. Next to each phonon dispersion curves, the corresponding total PhDOS, partial PhDOS due to interface (containing two Ge atoms, four Te atoms), and their partial PhDOS along the <001 > direction are shown. Fig. 2 shows that compared with the total PhDOS, the contribution rate of GTBT superlattice structure's partial PhDOS due to interface is significantly small in lower frequencies range, the same phenomenon can be found along the <001 > direction, these obviously indicate Bi atoms' impact on interface and the strong interface scattering of GTBT, which would result in small phonon group velocity and finally bring decrease in lattice thermal conductivity. Meanwhile, the result shows the Γ–A direction, owing ultra-flattened phonon dispersion curves, differs significantly from the other directions, this indicates the anisotropic phonon group velocity of superlattice materials, and ultimately results in anisotropic lattice thermal conductivity. Additionally, we can find the PhDOS of GTBT superlattice is divided in two ranges: 0–2.49 THz and 2.49–5.40 THz, which frequencies are lower than the PhDOS of GTST with two ranges 0–2.64 THz and 2.64–5.59 THz. This phenomenon leads to a little bigger heat capacity for GTBT superlattice according to the eqn (3) given below, and it have an adverse slightly impact on the decrease of the lattice thermal conductivity. The results of superlattice structures with the other three phases display the same phenomenon as the inverted Petrov phase.
In order to study how the changes of phonon group velocity and heat capacity effect on the thermal conductivity. We obtained the thermal conductivity from the calculated phonon spectrum and PhDOS. The theory we employed here is classical theories of thermal conductivity, lattice thermal conductivity is expressed as,21
(1) |
(2) |
(3) |
Relaxation time's inverse can be given by contributions from various scattering mechanisms:22
(4) |
The first term stands for boundary scattering, and the second term is an empirical formula of U process. Here, D stands for size of ideal crystal, ωm stands for the highest frequency in a phonon dispersion relation and B is a fitting parameter.
The lattice thermal conductivities of GTBT superlattice materials are calculated based on the above calculations, as can be seen in Fig. 3. We found the lattice thermal conductivity is strongly temperature dependent, being attributed to significant contribution from U process, which is related to the phonon dispersion curves.23
Fig. 3 Lattice thermal conductivity of GTBT and GTST superlattice structures as a function of lattice temperature calculated. |
Fig. 3 also obviously show the order of lattice thermal conductivities is Kooi > Petrov > Ferro-GeTe > inverted Petrov phase for GTBT superlattice materials, which is in line with the order of group velocity discussed in Fig. 1. This proves that while the strength of interfaces' effect becomes strong, the lattice thermal conductivities of superlattice materials will decrease. And the results of calculations demonstrate the lattice thermal conductivities of GTBT superlattice materials are smaller than GTST superlattice materials, for Kooi, Ferro-GeTe, and inverted Petrov phase, respectively. This phenomenon confirms Bi atoms in superlattices have a positive impact on reducing the lattice thermal conductivity. Meanwhile, we found the lattice thermal conductivity of GTBT superlattice with Petrov phase is a little bigger than the corresponding GTST superlattice structure. For GTBT superlattice with Petrov phase, both two Bi atoms are away from the interface, which would weaken Bi atoms' impact on the interface, and result that group velocity of GTBT with Petrov phase is only a slightly smaller than GTST with Petrov phase. Since GTBT's bigger heat capacity, Petrov phase present different change trend from other phases because of group velocity's and heat capacity's effect in combination, as shown in eqn (1). Despite this, the thermal diffusivity of GTBT superlattice with Petrov phase will still decrease, because the thermal diffusivity α = k/(ρC), and this is helpful to suppress the thermal crosstalk problem. This is in line with our expectation, namely proposing Bi-based phase change superlattice materials to reduce programming current and suppress the thermal crosstalk between adjacent storage units in PCM.
To verify the above change trend of GTBT superlattice materials' lattice thermal conductivity, we measured the thermal conductivity of GeTe/Bi2Te3 superlattice-like film materials by 3ω method. The 3ω method is a well-established method for measuring the thermal conductivity of a thin film.24 The GeTe/Bi2Te3 superlattice-like film materials are formed by alternately depositing GeTe and Bi2Te3, and interfaces are formed between two different chalcogenide material layers. The total thicknesses of all films are kept 150 nm and the thickness ratio of GeTe to Bi2Te3 is kept at 2:1, the number of interfaces N is controlled by varying the period length of each cycle. Fig. 4 shows the measured thermal conductivities of GeTe/Bi2Te3 superlattice-like materials with total thicknesses 150 nm and different number of interfaces (N). It exhibits GeTe/Bi2Te3 superlattice-like materials of all numbers of interfaces show a lower thermal conductivity than the GeTe/Sb2Te3 superlattice-like materials, and reach an extremely low thermal conductivity at 0.162 W mK−1. This drop is in accordance with our calculated results, and proves GeTe/Bi2Te3 superlattice materials are promising candidates to reduce the thermal conductivity of phase-change materials. Additionally, we found an interesting phenomenon that a minimum thermal conductivity occurs in the process of increasing N, which is probably because the phonon exhibits wavelike behaviour when the period length of superlattice-like materials is shorter than the phonon mean free path, as reported by Simkin et al.25
This journal is © The Royal Society of Chemistry 2019 |