N. Rajaa,
D. Muralib,
S. V. M. Satyanarayanaa and
M. Posselt*c
aDepartment of Physics, Pondicherry University, Puducherry 605 014, India
bIndian Institute of Information Technology Design and Manufacturing, Kurnool, Andhra Pradesh 518002, India
cHelmholtz-Zentrum Dresden-Rossendorf, Institute of Ion Beam Physics and Materials Research, Bautzner Landstraβe 400, 01328 Dresden, Germany. E-mail: m.posselt@hzdr.de
First published on 23rd October 2019
The temperature dependence of the stability of bulk BaZrO3 (BZO) and of the vacancies in this material are investigated by considering phonon contributions to the free energy. The stability diagram of BZO is determined for different chemical environments. With increasing temperature the stability region becomes smaller which is particularly caused by the strong temperature dependence of the chemical potential of gaseous oxygen. The free formation energy of Ba, Zr, and O vacancies in BZO is calculated for all possible charge states and for different atomic reservoirs. While the free formation energy of Zr vacancies is strongly influenced by temperature a weaker dependence is found for Ba and O vacancies. This also has an effect on the charge transition levels at different temperatures. The present results demonstrate that O poor reservoir conditions and a Fermi level close to the valence band maximum favour a high concentration of doubly positively charged O vacancies which is a prerequisite to get a large number of protonic defects and good proton conductivity. In such a chemical environment the number of Ba and Zr vacancies is low so that Ba and Zr deficiencies are not an important issue and BZO remains sufficiently stable.
(1) |
Oxygen vacancy concentration in BZO can be increased by various techniques like strain engineering, doping, etc. Doping of BZO with lower valence cations such as Y can essentially improve the proton conductivity.12–14
First principles Density Functional Theory (DFT) calculations can contribute to the understanding of the promising properties of BZO. Recently, the stability of bulk BZO and of Ba, Zr, and O vacancies at ground state has been extensively studied by DFT methods.15 Since solid-state proton conductors such as BZO operate at relatively high temperatures, it is also very important to investigate the thermodynamic stability of the differently charged vacancy defects in dependence on the chemical environment. Sundell et al.16 used DFT to study the neutral and fully charged Ba, Zr and O vacancies in the ground state and determined the temperature dependence of the formation of neutral and doubly positively charged O by thermodynamic modelling. In a previous DFT work we found that at 1000 K phonon contributions increase the migration barrier of the doubly positively charged oxygen vacancy by 0.35 eV.17 Bjørheim et al. investigated the neutral and the doubly positively charged state of the O vacancy at finite temperatures and found that near the conduction band minimum the phonon contribution decreases the free formation energy of the neutral vacancy by around 0.8 eV at 1000 K, but does not alter the free formation energy of the doubly positively charged O vacancy.18 However, in this study only the O poor chemical environment was considered. The absorption of CO2 at high temperature was investigated in pristine as well as Y doped BZO by Polfus et al. and the role of Ba, Zr, and O vacancies was discussed.19 Recent experimental studies clearly indicate that considerable Ba deficiency may occur at high temperatures.20 This leads to a drastic decreases of proton conductivity21 and material stability.22 Cation vacancy defects influence the site occupancy of foreign atoms and dopants.23,24 In this context, it is very important to determine the properties of the Ba vacancy at high temperatures. Also the Zr vacancies are responsible for the electrochemical properties and the thermodynamic stability of BZO. It is therefore important to study the temperature dependence of the free formation energy of all the possible vacancies in BZO, for different charge states and various atomic reservoir conditions. To the best of our knowledge, such comprehensive investigations have not been performed yet.
In this work, a systematic first-principles study on the thermodynamic stability of Ba, Zr, and O vacancies in BZO is performed. In the first part, the thermodynamic stability of BZO is determined in dependence on temperature and on the chemical potentials of atomic reservoirs, which are in equilibrium with BZO, i.e. on different conditions of BZO synthesis. The free formation energy of neutral and charged Ba, Zr, and O vacancies and the corresponding charge transition levels are calculated in the second part, with particular emphasis on the influence of Fermi level, chemical environment, and temperature. In this manner, conditions for the preferential formation of doubly positively charged O vacancies and for the limitation of the number of Ba and Zr vacancies can be identified. These conditions are important prerequisites for achieving optimum proton conductivity in BZO.
Table 1 demonstrates that the above mentioned choice of VASP input data yields reasonable values for ground state structural properties of solid Ba, Zr, BaO, ZrO2, and BZO, and the O2 molecule.
This work | Theory | Experiment | |
---|---|---|---|
Ba (BCC) | |||
a (Å) | 5.039 | 4.770 (ref. 30) | 5.020 (ref. 31) |
Zr (HCP) | |||
a (Å) | 3.220 | 3.229 (ref. 32) | 3.232 (ref. 27) |
c/a | 1.732 | 1.600 (ref. 25) | 1.592 (ref. 27) |
O (dimer) | |||
r0 (Å) | 1.215 | 1.22 (ref. 25) | 1.21 (ref. 26) |
BaO (cesium chloride) | |||
a (Å) | 5.515 | 5.576 (ref. 15) | 5.539 (ref. 28) |
ZrO2 (monoclinic) | |||
a (Å) | 5.194 | 5.217 (ref. 15) | 5.151 (ref. 29) |
c/a | 1.039 | 1.034 (ref. 15) | 1.032 (ref. 29) |
BaZrO3 (cubic) | |||
a (Å) | 4.269 | 4.208 (ref. 15) | 4.192 (ref. 30) |
The frozen phonon approach and the harmonic approximation33,34 are applied to determine the vibrational frequencies which are used to investigate the effect of temperature on the materials properties. In these calculations, ground state atomic positions are slightly displaced (by 0.015 Å) in positive and negative x-, y- and z-directions to obtain the respective force derivatives for the dynamical matrix. The symmetry of the underlying supercell is used to reduce the number of atomic displacements and thus computational costs. The diagonalization of the dynamical matrix yields all vibrational frequencies ωi of the supercell. All the calculations are performed for the gamma point in the space of the phonon wave vectors. At a given temperature T the phonon or vibrational contribution Gvib(T) to the Gibbs free energy of a system of N atoms is defined by
(2) |
(3) |
(4) |
ΔfHZrO2 = EZrO2 − EZrhcp − EO2 | (5) |
While DFT is able to determine rather precise values for the ground state energies of BZO, BaO, ZrO2, Ba, and Zr, this method yields poor data for the ground state energy of the O2 molecule. Wang et al.39 attributed this to the over binding caused by treatment of exchange and correlation effects by the GGA. These authors also found that this issue leads to a difference of about 1.36 eV (per O2 molecule) between theoretical and experimental data for the oxidation energy of many metal oxides. Therefore, in the present work this value is added to the DFT value for EO2 which corresponds to the procedure proposed by Wang et al.39 This correction was also used by Bjørheim et al. in the calculation of the free formation energy of the oxygen vacancy.18
The data obtained for the formation energy of BZO, BaO and ZrO2 are −18.46 eV, −4.98 eV and −11.03 eV, respectively. These data are slightly different to previously reported ground state DFT results of −16.73 eV (ref. 16) and −17.82 eV (ref. 15) for BZO, −5.17 eV (ref. 16) and −5.55 eV (ref. 15) for BaO, and −10.25 eV (ref. 16) and −10.27 eV (ref. 15) for ZrO2, since in these papers the O2 correction was not taken into account.
The vibrational contribution to the Gibbs free energy of formation per formula unit is given by
(6) |
(7) |
(8) |
Fig. 1 Gibbs free energy of formation of BaO, ZrO2 and BZO per formula unit, in comparison with reported data obtained from experiments and thermodynamic modelling.40–42 |
For all three compounds the absolute value of the Gibbs free energy of formation decreases if the temperature increases. There is a very good agreement between calculated and experimental data at lower temperatures. The discrepancy arising at high temperatures may be explained by anharmonic effects that are not taken into account in the calculation. The contribution of zero-point vibrations to the Gibbs free energy of formation is −0.16 eV, −0.67 eV and −0.53 eV for BZO, BaO and ZrO2 respectively. Therefore, at 0 K the Gibbs free energy of formation is −18.62 eV (BZO), −5.65 eV (BaO), and −11.56 eV (ZrO2), which is in good agreement with the thermochemical reference data of −18.27 eV (ref. 40), −5.68 eV (ref. 41), and −11.41 eV (ref. 42) for BZO, BaO and ZrO2, respectively. This also demonstrates that the correction of the ground state energy EO2 (see above) leads to consistent results.
The Gibbs free energy of formation of BZO (per formula unit) from BaO and ZrO2 is defined similarly to eqn (3)–(8)
(9) |
Fig. 2 shows that the absolute value of this quantity decreases with temperature, i.e. the probability of dissociation of BZO into BaO and ZrO2 increases. This trend is in agreement with experimental results.43 The quantitative difference at higher temperature may be due to anharmonic effects, which are not considered in the present work. The difference between the ground state value of ΔfGBaZrO3 and that for 300 K is −1.34 eV, which is in good agreement with the experimental values of −1.33 eV and −1.19 eV at 300 K.43,44
Fig. 2 Gibbs free energy of formation of BZO (per formula unit) from BaO and ZrO2 as a function of temperature. |
Fig. 1 and 2 clearly demonstrate the importance of vibrational effects on the thermodynamic stability of BZO, BaO and ZrO2.
μi = μi0 + Δμi | (10) |
Here, the quantities μi0 are the chemical potentials of Ba, Zr, and O atoms in their standard solid (Ba, Zr) and gaseous (oxygen) reference states.
The stability of BZO is investigated by imposing constraints on Δμi. For example, the set of constraints that do not allow BZO to decompose into elements Ba, Zr and O2 is given by
ΔμBa ≤ 0, ΔμZr ≤ 0 and ΔμO ≤ 0 | (11) |
Further, constraints that do not allow BZO to decompose into binary oxides BaO and ZrO2 are governed by
ΔfGBaO ≥ ΔμBa + ΔμO | (12) |
ΔfGZrO2 ≥ ΔμZr + 2ΔμO | (13) |
These constraints together with the following equation allow us to compute the stability diagram, where the suitable chemical environment for the formation of BZO can be determined.
ΔfGBaZrO3 = ΔμBa + ΔμZr + 3ΔμO | (14) |
Fig. 3 represents the stability diagram of BZO with the competing binary oxides BaO and ZrO2. Points A, B, C, D and X represent five different chemical potential conditions at 0 K. These conditions are obtained from eqn (10)–(14) and using the corresponding values for the Gibbs free energy of formation at 0 K. Points A and B correspond to O rich conditions with the chemical potential value ΔμO = 0 eV. At point C the environment is Zr rich, at point D, Ba rich. The condition of extreme reduction can be obtained at point C, where the chemical potential of oxygen is most negative: ΔμO = −5.78 eV. Point X is in the intermediate stability region of BZO between oxidation and reduction conditions.
Fig. 3 can be compared with the results obtained by Abbas et al.15 They calculated the stability diagram for the ground state using all electron calculation (WIEN2k code) and did not include the O2 correction (see above). Comparison of our ground state chemical potential values of Ba, Zr, and O with the literature data may helpful to understand the significance of O2 correction. For example, at point C, O poor/Zr rich conditions, the atomic chemical potential values for the ground state obtained from our calculation is −1.96 (ΔμBa), 0.00 (ΔμZr) and −5.50 (ΔμO), which is slightly different from the literature values of −2.423 (ref. 15), 0.000 (ref. 15) and −5.134 (ref. 15) for ΔμBa, ΔμZr, and ΔμO respectively. The deviations are mainly due to the inclusion of the O2 correction, but certainly also due to the use of a pseudopotential in the VASP calculations. At other points of the stability diagram similar differences between our ground state values of the chemical potential and the corresponding data of Abbas et al.15 occur.
As the temperature increases, the region of chemical stability of BZO becomes smaller. This is due to the temperature dependence of the Gibbs free energies of formation ΔfGBaZrO3, ΔfGBaO, and ΔfGZrO2. At 1000 K the stability region of BZO is limited by the points A′, B′, C′, 0, and D′. At points D′ and C′ the chemical potential of oxygen is −4.83 eV and −4.98 eV, respectively. This drastic change compared to 0 K is due to the high entropy of the gaseous O2 molecule, which leads to a relatively fast decrease of the absolute value of the corresponding free energy if temperature increases. The strong temperature dependence of ΔμO is also the cause for the loss of the stability of BZO as well as BaO and ZrO2 by the release of oxygen, which occurs in regions that correspond to strong oxidation conditions at 0 K. Point X′ in the intermediate stability region is obtained by shifting point X towards point 0, by a distance corresponding to the difference between A and A′ or B and B′. On the other hand, the boundaries between the stability regions of BZO and BaO and those of BZO and ZrO2 change relatively weakly if the temperature is increased.
It should be mentioned that the relation between the chemical potential μi and the atomic concentration Ci is given by
(15) |
The partial oxygen pressure pO2 can be obtained from the chemical potential μO using
(16) |
ΔEf(Viq) = Etot(Viq) − Etot(bulk) + q(EVBM + Ef) + μi | (17) |
At temperature T the Gibbs free formation energy of a vacancy is defined similarly to eqn (17)
ΔGf(Viq,T) = Gtot(Viq,T) − Gtot(bulk,T) + q(EVBM + EF) + μi(T) | (18) |
The solid lines in Fig. 4 depict the free formation energies of vacancies at 0 K for reservoir conditions corresponding to points A, B, C, D and X of the stability diagram (Fig. 3), whereas the dashed lines are the data for 1000 K and for points A′, B′, C′, D′, and X′. In dependence on the Fermi energy neutral or charged vacancies are energetically favored. In the case of points A and A′ the charge transitions are illustrated in detail in Fig. 4b. Because of eqn (17), the Fermi level at which the charge transitions occur is independent of reservoir conditions, but the transition level depends on temperature. It should be noticed that for a given Fermi energy the diagrams show only values for the lowest free formation energy among all the possible charge states. Close to the VBM the O vacancy has the lowest free formation energy while the free formation energy of Ba and Zr vacancies is highest. The opposite behavior is found near the conduction band minimum (CBM). The values of the free formation energy strongly depend on the reservoir conditions. At points C and C′ as well as at D and D′ (oxygen poor conditions) the most stable defect is the O vacancy in the +2 charge state if the Fermi level is closer to VBM than to CBM. For other values of EF the negatively charged Ba and Zr vacancies are more stable. Under O rich conditions (points A and A′, B and B′) Ba and Zr vacancies are more stable than the O vacancy, for all possible values of the Fermi energy. Near VBM these vacancies are preferentially neutral, towards the CBM they are negatively charged. In the case of the Ba and the O vacancy the difference between the data obtained for 0 and 1000 K is dependent on the value of EF, in contrast to the Zr vacancy where such a dependence is not significant while the absolute value of the difference is higher.
Fig. 4 Gibbs free formation energies of Ba (green), Zr (blue) and O (red) vacancies at 0 K (solid line) and 1000 K (dashed line), as function of Fermi energy, for different chemical environments (see Fig. 3). |
For O poor/Zr rich conditions, i.e. at point C, the ground state formation energy obtained from our calculation is 5.39 eV (VBa0), 14.56 (VZr0), and −3.43 (VO2+), whereas Abbas et al.15 obtained is 5.66 eV, 16.30 eV and −1.84 eV for VBa0, VZr0 and VO2+ respectively. Again, the differences are mainly due to the O2 energy correction applied in this work (see above).
Fig. 5 summarizes the data of the free formation energy of Ba, Zr, and O vacancies at 0 and 1000 K for the case that the Fermi level is at the VBM. The stability of the Ba vacancy is highest at points B and B′ i.e. at O rich conditions, and the neutral charge state is most favored. On the other hand, at points D and D′, i.e. at Zr rich conditions, the free formation energy of the Ba vacancy is highest. The Zr vacancy shows a behavior similar to that of the Ba vacancy but has its minimum free formation energy at points A and A′. The stability of the Zr vacancy increases significantly with temperature: while at 0 K the most probable state (points A and A′) has a positive free formation energy (1.00 eV) this quantity is negative at 1000 K (−0.88 eV). Neither the Ba nor the O vacancy shows such a strong T dependence since in these cases the vibrational contributions to the free formation energy are lower. At and near the VBM the oxygen vacancy is most stable at points C and C′ as well as at points D and D′ whereby the doubly positively charged state is preferred. This condition favors the production of protonic defects according to reaction (1). The results depicted in Fig. 4 and 5 clearly show that the reservoir conditions at points C (C′) and D (D′) favor a high concentration of doubly positively charged O vacancies and a low concentration of Ba and Zr vacancies. This is an optimum prerequisite in order to achieve high proton conductivity in BZO while avoiding much Ba and Zr deficiencies. As shown in a previous work17 phonon contributions increase the migration barrier of the doubly positively charged O vacancy. This contributes to the high-temperature stability of BZO observed in experiments.
Fig. 5 Free formation energy of Ba, Zr and O vacancies at the valence band maximum (VBM), for different points of the stability diagram (see Fig. 3). Data for 0 K and 1000 K data are shown by solid and dashed lines, respectively. |
As already mentioned above, the charge state of Ba, Zr, and O vacancies changes with increasing Fermi energy. A diagram representing all possible charge transitions of Ba, Zr and O vacancies calculated at 0 K and 1000 K is given in Fig. 6. As the Fermi level increases the Ba vacancy undergoes a charge transition from 0 to −1 to −2, whereas the Zr vacancy exhibits a transition from 0 to −1 to −2 to −3 to −4, and the O vacancy undergoes transitions from +2 to +1 to 0. At 1000 K the charge transitions occur at lower values of EF than at 0 K. The influence of temperature on the Fermi level of the charge transition is highest for the Zr vacancy. In this case at 1000 K the range of charge state −1 is extended compared to 0 K whereas the charge state −2 is not stable so that a direct transition between −1 and −3 takes place. For O vacancies, transition levels were found closer to CBM than for the other vacancies. At 0 K the (0/+) and the (+/2+) transitions occur at a distance of 0.46 and 1.43 eV from CBM, respectively. On the other hand, at 1000 K the first and the second transition takes place at 1.15 eV and 1.77 eV, respectively, i.e. the range where the doubly positively charged O vacancy is stable is slightly smaller than at 0 K.
This journal is © The Royal Society of Chemistry 2019 |