Milan
Schirowski‡
a,
Christoph
Tyborski
b,
Janina
Maultzsch
bc,
Frank
Hauke
a,
Andreas
Hirsch
*a and
Jakub
Goclon‡
*d
aChair of Organic Chemistry II & Joint Institute of Advanced Materials and Processes, Friedrich-Alexander University of Erlangen-Nürnberg, Nikolaus-Fiebiger-Straße 10, 91058 Erlangen, Germany. E-mail: andreas.hirsch@fau.de
bInstitut für Festkörperphysik, Technische Universität Berlin, Hardenbergstraße 36, 10623 Berlin, Germany
cChair of Experimental Physics, Friedrich-Alexander University Erlangen-Nürnberg, Staudtstr. 7, 91058 Erlangen, Germany
dInstitute of Chemistry, University of Bialystok, Ciolkowskiego Str. 1K, 15-245 Bialystok, Poland. E-mail: j.goclon@uwb.edu.pl
First published on 22nd October 2018
The reaction of neutral single-walled carbon nanotubes (SWCNTs) with diazonium salts proceeds with a high selectivity towards metallic carbon nanotube species; this reaction is well-understood and the mechanism has been elucidated. In the present joint theoretical and experimental study, we investigate the reaction of negatively charged SWCNTs – carbon nanotubides – with diazonium salts. Our density functional theory calculations predict a stronger binding of the aryl diazonium cations to charged metallic SWCNTs species and therefore lead to a preferential addend binding in the course of the reaction. The Raman resonance profile analysis on the reductive arylation of carbon nanotubides obtained by the solid state intercalation approach with potassium in varying concentrations confirms the predicted preferred functionalization of metallic carbon nanotubes. Furthermore, we were also able to show that the selectivity for metallic SWCNT species could be further increased when low potassium concentrations (K:C < 1:200) are used for an initial selective charging of the metallic species. Further insights into the nature of the bound addends were obtained by coupled thermogravimetric analysis of the functionalized samples.
In order to elucidate the underlying driving forces for an electronic type selective reaction of carbon nanotubides we reduced the amount of parameters by charging the SWCNTs with the alkali metal potassium in a clean and controllable solid state reaction.23,24 The alkali metal concentration can be varied and has a direct influence on the final degree of functionalization. Moreover, in a previous joint experimental and theoretical investigation, we were able to show that for low K:C ratios of <1:200 the adsorption of a potassium atom on metallic carbon nanotubes is always preferred over the adsorption on semiconducting tubes, independently of the tube diameter.29 In principle, this selective charging of metallic carbon nanotubes in the low charge density regime can be exploited for a charge-driven separation approach. On the other hand, in typical functionalization experiments27 vastly higher potassium:carbon charging ratios are used and therefore any observed electronic type selective arylation and alkylation of nanotubide intermediates cannot simply be referred to a selective charging of specific helicities in the starting mixture.
Identifying the selectivity-determining step of the reaction is a challenging task which can hardly be solved by an experimental approach only. Consequently, in order to understand the underlying principles of electronic type selective SWCNT reactions, we focused in our present study on the well-defined reaction of a diazonium cation with solid state charged carbon nanotubes. The advantage of this protocol is the absence of further co-reducing agents such as liquid ammonia or naphthalene, which would severely obstruct a comparison of the experimental data with the theoretical predictions. Based on a density functional theory (DFT) approach, in the present work we investigated the direct interaction of the electrophilic trapping reagent with the negatively charged carbon nanotubides of both electronic types. We could verify that aryl diazonium cations bind stronger to charged metallic species than to semiconducting ones. Moreover, a higher density of states of SWCNTs in the vicinity of the singly occupied molecular orbital/lowest occupied molecular orbital (SOMO/LUMO) of the aryl diazonium radical/cation pair – i.e. higher charging density – directly leads to a more efficient electron charge transfer from the charged nanotubides to the adsorbed electrophilic trapping reagent.13 In addition, the calculations reveal no correlation of the PhN2 radical/cation-SWCNTs interaction energy with varying tube diameters. Based on these theoretical results, charged metallic SWCNTs should be more reactive than their semiconducting counterparts, which is in perfect agreement with the results we obtained on Birch type reduced systems.27 In the present experimental approach, we carried out the SWCNT reduction in a well-defined potassium intercalation30 protocol with a variation of the applied charge density in the course of the reductive diazotation reaction (Scheme 1).29 The successful arylation of the carbon nanotubes was verified by a thermogravimetric (TG) product analysis, coupled with gas-chromatographic (GC) separation and mass-spectrometric (MS) characterization (TG-MS and TG-GC-MS). Moreover, by in-depth Raman analysis of the RBM (radial breathing mode) region of the covalently functionalized carbon nanotubes, we could prove that the reductive diazotation leads to a preferred functionalization of metallic SWCNT species, as predicted by our DFT calculations, and that at potassium concentrations below the 1:200 threshold the selectivity for metallic carbon nanotubes could be increased in a cooperative utilization of two selectivity-determining parameters.
Scheme 1 Arylation of reductively exfoliated carbon nanotubides, obtained by a solid state intercalation process with potassium (K:C ratio of 1:4) by electrophilic trapping with benzenediazonium cations. Three samples SWCNT–Phn:1(KC4) (n = 1, 4, 20) were synthesized with varying diazonium:nanotube carbon ratios (1:1, 4:1, and 20:1) – see also Table 2. |
SWCNT | n | l opt/Å | d/Å | k-point |
---|---|---|---|---|
(10,0) | 160 | 17.14 | 7.89 | 1 × 1 × 4 |
(9,4) | 532 | 49.26 | 9.06 | 1 × 1 × 1 |
(7,5) | 436 | 44.61 | 8.25 | 1 × 1 × 1 |
(8,3) | 388 | 42.07 | 7.75 | 1 × 1 × 1 |
(6,6) | 168 | 17.27 | 8.21 | 1 × 1 × 4 |
(13,4) | 316 | 21.94 | 12.08 | 1 × 1 × 2 |
(13,1) | 244 | 19.26 | 10.66 | 1 × 1 × 2 |
(12,3) | 252 | 19.60 | 10.84 | 1 × 1 × 2 |
The other functionalized SWCNT–PhC:Ph(KCx) samples were synthesized via the same procedure, only altering the molar amounts of potassium and diazonium salt according to Table 2.
Sample | n (K)/mmol | n (diaz.)/mmol | Ratio K:diazonium |
---|---|---|---|
SWCNT–Ph(1:1)(KC4) | 0.13 | 0.50 | 1:4 |
SWCNT–Ph(4:1)(KC4) | 0.13 | 0.13 | 1:1 |
SWCNT–Ph(20:1)(KC4) | 0.13 | 0.025 | 5:1 |
SWCNT–Ph(10:1)(KC200) | 0.0025 | 0.050 | 1:20 |
Raman measurements for the in-detail screening of the RBM modes were performed in backscattering geometry under standard ambient conditions. An Ar+/Kr+ and an Ti:Sa laser were used to tune the excitation energies between 1.50 eV and 2.73 eV. Laser power was kept below 0.6 mW at all times. The tunable laser setup allowed to probe metallic M11, as well as semiconducting S22, S33, and S44 electronic transitions with diameters between ∼7 and 13 Å. Raman spectra were taken with a Dilor XY800 triple monochromator and a neon lamp was used for frequency calibration. A final assignment of SWCNTs in the sample was carried out via pattern recognition.39–41 For further details, a full characterization of another HiPco sample can be found in the literature.39,42
Thermogravimetric analysis coupled with mass spectrometry: TG-MS (online) was performed on a Netzsch Skimmer STA 409 CD instrument with a quadrupole in EI+ mode. Samples were heated with a constant rate of 20 K min−1 from room temperature to 700 °C under a constant flow of helium (80 mL min−1).
Thermogravimetric analysis coupled with gas chromatography and mass spectrometry: TG-GC-MS was performed on a Pyris 1 TGA from Perkin-Elmer coupled with a Clarus 680 gas chromatograph with an Elite-5 column and an SQ 8 quadrupole mass spectrometer. Samples (2–4 mg) were heated with a constant rate of 20 K min−1 from room temperature to 700 °C. Helium with a constant flow of 1 mL min−1 was used as carrier gas. Injection for the detection of covalently attached aryl moieties was performed at 280 °C, for the decomposition products of SWCNT–Ph(20:1)(KC4) at 480 °C (temperatures determined by TG-MS results). The GC temperature ramp was 40–280 °C with a constant heating rate of 10 K min−1 and a final 10 min plateau at the maximum temperature. The obtained data was processed with TurboMass software and bibliographic searches where carried out with NIST MS Search 2.0.
SWCNT type | Cfs–N [Å] | C⋯C [Å] | E b [eV] | |
---|---|---|---|---|
L | II | L | II | |
(10,0) | 1.58 | 3.28–3.50 | 2.77 | 3.61 |
(9,4) | 1.59 | 3.27–3.49 | 2.55 | 3.53 |
(7,5) | 1.59 | 3.26–3.52 | 2.53 | 3.44 |
(8,3) | 1.58 | 3.37–3.58 | 2.60 | 3.44 |
(6,6) | 1.56 | 3.28–3.51 | 2.71 | 3.45 |
(13,4) | 1.64 | 3.19–3.55 | 2.88 | 3.97 |
(13,1) | 1.60 | 3.27–3.55 | 2.80 | 3.80 |
(12,3) | 1.60 | 3.10–3.43 | 2.70 | 3.33 |
The parallel arrangement (II) of the benzenediazonium cation and the charged SWCNTs originates from van der Waals type mutual interactions. The initial PhN2+ has been transformed into the radical with the N–N bond distances and the N–N–C angles of 1.19 Å and 125.5°, respectively. The obtained structural parameters are similar to those obtained for the radical structure in the gas phase (see Fig. S3†). The shortest C–C distances between the aryl group and the SWCNT are in the range of 3.10 to 3.58 Å (see Table 3), which suggests the dominant role of the π–π stacking interactions. This is in agreement with the results of the DFT(PBE)+D2 calculations for non-covalently functionalized SWCNTs with other aromatic molecules.45
Apart from the structural parameters, the reactivity of the systems was also analyzed in terms of its energetic properties. The binding energy (Eb) between the benzenediazonium cation (PhN2+) and the charged nanotubide (SWCNT−) can be quantified by eqn (1):
Eb = (ESWCNT− + EPhN2+) − ESWCNT–PhN2 | (1) |
The binding energies (Eb) are very high because of the unbalanced charge of the individual components, therefore, only the relative values should be compared. Since the SWCNTs− anion with attached PhN2+ cation contain an odd number of electrons in the supercell, both spin-polarized and spin-unpolarized schemes were included in the computational setup. For the perpendicular arrangements (L) the singlet and doublet state yields almost the same binding energy, whereas in the parallel case (II) the doublet state is always energetically favourable, unambiguously showing the formation of the PhN2 radical on the nanotube sidewalls. However, it may happen that the energy difference between the singlet and the doublet state is small, like for the m-(12,3)–PhN2 (II) arrangement, namely −0.03 eV. Such small energy difference makes the discussion about the stability of the system hard due to the limited accuracy of the DFT. Here, the analysis of the structural parameters of the attached PhN2 group shows its similarity to the structure of PhN2+ in the gas phase.
The computed binding energies (Eb) are on average higher for both types of the arrangement for the metallic nanotubes, with the maximum differences of about 0.3–0.5 eV. The results obtained by Sumpter et al.46 for interactions between the aryl diazonium cation and neutral SWCNTs for the perpendicular (L) arrangement also show the enhanced stability for the interaction with metallic SWCNT species. In such cases, the increase of the Cfs-N bond length with increasing nanotube diameter is observed (see Tables 1 and 3). Regardless of the diameters, the parallel arrangement (II) is energetically favored by 0.7–1.1 eV in comparison to the perpendicular (L) one. The binding energies (Eb) obtained do not depend on the nanotube diameter but rather on the chirality type. This is similar to the results obtained by Umeyama et al.47 for the attachment of a single 4-(1-pyrenyl)phenyl radical on the SWCNTs sidewalls of various chiralities. Furthermore, it has been shown46 that if the diazonium salt anion (BF4−) is included in the calculations, there is a large preference for PhN2+ to associate with it, instead of being deposited on the surface of the carbon nanotube. Taking into account the presence of the BF4− anion in the smallest conjugates, namely sc-(10,0)/m-(6,6)–PhN2, with the perpendicular arrangement (L), the formation of the PhN2⋯BF4− complex on the nanotube sidewall (Eb of 2.61/2.39 eV) is observed (Fig. 1b). Therefore, we can conclude that the diazonium salts interact primarily with SWCNTs via van der Waals interactions before the N2 is released and the aryl radical is formed.
The reduction of the diazonium cation in the course of an electron transfer reaction and subsequent radical formation is the rate-limiting step. Electron transfer occurs between any occupied state of the SWCNTs that matches in energy with an unoccupied state of the benzenediazonium cation. Such studies have previously been carried out for the functionalization of graphene with diazonium salts.48,49 By merging the electronic band structure with the chemical molecular orbital theory, the different reactivities of metallic and semiconducting SWCNTs can be explained. Fig. 2 shows the electronic structure (band structure and DOS) for the sc-(10,0)/m-(6,6)–PhN2 (II) conjugates. The results for the other SWCNT helicities under investigation are summarized in the ESI (Fig. S2).† The (6,6) carbon nanotube exhibits a metallic character (with a zero band gap) while the (10,0) tubes represent semiconducting species with a band gap of 0.8 eV. Significant differences in the DOS near the Fermi level are observed for the semiconducting and metallic systems. In the case of sc-SWCNTs–PhN2 conjugates, the appearance of a half-occupied non-dispersive band in the energy gap of semiconducting nanotubes is clearly seen. Fig. 3a presents the electron density of the Γ-point wave function of this band. This band corresponds to the singly occupied molecular orbital (SOMO) of the PhN2 radical that is mainly composed of the nitrogen orbitals (PDOS) (for details see Fig. S3†). The SOMO level always lies some distance from the top of the valence band of the sc-SWCNTs. Therefore, there is no overlap with the electronic states of the nanotube. In the case of the m-SWCNT–PhN2 conjugates, the SOMO is located about 0.25 eV below the Fermi level (see Fig. 2b and S3a†). As a result, the electron transfer should easily proceed between the charged m-SWCNT and the adsorbed cation. For the m-(12,3)–PhN2 conjugate (singlet state) a different electronic structure is observed (Fig. 3c). The attached PhN2 molecule retains the initial electronic configuration of the cation (the N–N bond distance of 1.13 Å and the N–N–C angle of 180.0°) where the lowest unoccupied molecular orbital (LUMO) (Fig. 3c and S3b†) is only partially occupied at the Fermi level. The common feature of the studied SWCNT–PhN2 systems is that metallic nanotubes have higher density of states (DOS) in the vicinity of the SOMO/LUMO of the benzenediazonium radical/cation.
Fig. 3 The electron density of the Γ-point wave function of the SOMO (a and b) and LUMO (c) of the aryl diazonium radical/cation for three different cases, see Fig. 2. The green surface represents an isovalue of 2 × 10−3 Bohr Å−3. |
From the experimental side, the electronic type selective arylation of intermediately charged carbon nanotubides has previously been reported for a Birch type reduction protocol with benzenediazonium tetrafluoroborate as trapping reagent.27 In this functionalization scenario, metallic carbon nanotubes were predominantly functionalized by the intermediately generated aryl radicals. In the present joint experimental and density-functional theory (DFT) study we investigated if the results obtained for the reductive diazotation under Birch type conditions can be transferred to other SWCNT reduction protocols. Simultaneously, we shed light on the underlying principles which determine the electronic type selectivity of the functionalization of carbon nanotubides with diazonium cations. Here, we focused on the reductive solid-state intercalation/charging of carbon nanotubes by potassium (Scheme 1) as the variation of the amount of reducing agent within the reductive activation step is one fundamental parameter to adjust the degree of functionalization in the respective SWCNT derivatives.23 The advantage of this charging protocol23,24,50 over alternative nanotubide generating approaches is the absence of further co-reducing agents such as liquid ammonia or naphthalene.17,20,25
Moreover, this solid state SWCNT activation protocol inherently allows to adjust the stoichiometric amounts of the reducing agent as well as that of the trapping electrophile over a wide range with high accuracy. For the generation of individualized, charged, and highly reactive nanotubide intermediates, we used the respective carbon nanotubide salt obtained by melting stoichiometric amounts of potassium with HiPco SWCNTs. The bronze-colored salt (KC4) was dispersed in absolute DMAc, yielding neatly dispersed carbon nanotubides. It has to be mentioned that strictly H2O- and O2-free solvents are mandatory for the successful reductive exfoliation and in order to suppress side reactions during the functionalization.23 The electrophilic trapping/functionalization sequence was carried out by the addition of varying amounts of benzenediazonium tetrafluoroborate in the potassium:diazonium ratios of 1:4, 1:1, and 5:1. After the addition of the diazonium compound the sample was worked up under aqueous conditions and characterized in detail by means of Raman spectroscopy and thermogravimetric analysis coupled to gas chromatography and mass spectrometry (TG-MS and TG-GC-MS).
It can be expected that based on a retro-functionalization mechanism,51 the highest excess of electrophilic trapping species should lead to the highest degree of functionalization and therefore an underlying electronic type selectivity should be easily detectable in the respective SWCNT–Ph(1:1)(KC4) derivatives, where a 4-fold excess of diazonium cations in relation to applied negative charges was used to quench the carbon nanotubides.
In carbon allotrope characterization, the intensity ratio of the D-mode in relation to the G-mode is commonly used as a measure for the amount of covalently bound addends in the functionalized samples, whereas the radial breathing modes (RBM) are characteristic features for the individual SWCNT chiral indices present in the mixture. Their position in the spectrum only depends on the diameter and on the applied laser excitation energy.52–54
The mean Raman spectra of the arylated SWCNT derivatives, probed with a laser excitation energy of 2.33 eV, are plotted in Fig. 4 – the spectral information obtained with a laser excitation energy of 1.58 eV is presented in Fig. S4;† spectral data for 14 further excitation energies in the range between 1.59 eV–2.71 eV are presented in the ESI (Fig. S5–S8: RBM region, Fig. S9–S11: D-/G-band region).† Based on the bulk analysis of the obtained ID/IG intensity ratios (based on statistical mean of peak amplitude quotients, s. Table S1†) it becomes evident that, as expected, the highest degree of functionalization (ID/IG = 0.97) is obtained for SWCNT–Ph1:1(KC4) with the highest diazonium excess in relation to applied negative charges (4:1), whereas for SWCNT–Ph20:1(KC4) with a diazonium to charge ratio of 1:5 the lowest degree of functionalization with an ID/IG ratio of 0.17 is obtained.
An additional indication for successful addition and a viable feature to probe preferential functionalization of certain nanotubes to a particular tube type is the decrease of RBM intensity. The high concentration of covalently bound addends in SWCNT–Ph1:1(KC4) leads to an almost complete depletion of the characteristic RBM signature (inset Fig. 4) and, therefore, we focused our electronic type selectivity investigation of the reductive diazotation reaction on sample SWCNT20:1(KC4) where the RBM fine structure of the spectrum is preserved after the covalent addend binding. Analysis of the Raman resonance profiles allows for the determination of the nanotube indices (n,m) within the ensemble.39,41,55 This in turn gives the opportunity to choose distinct laser excitation energies addressing either exclusively metallic nanotube families, or exclusively semiconducting ones, or both of them. Thereby, we have a tool to selectively analyze the influence of a functionalization on certain families of carbon nanotubes.
For our HiPco SWCNT batch we have predominantly found carbon nanotubes with diameters of around 10 Å. Hence, we address semiconducting tubes with excitation energies between 2.73 and 2.55 eV belonging to the families (2n + m = constant) 23S and 26S. Between 2.55 eV and 2.30 eV we probe both semiconducting 29S and 32S as well as metallic 21M and 24M carbon nanotubes, whereas around 2.2 eV only metallic 24M and 27M carbon nanotubes are probed. Lower excitation energies will again bring semiconducting tubes in resonance exhibiting larger diameters compared to the metallic tubes in resonance. At laser excitation energies around 1.9 eV, 27M and 30M metallic as well as 23S semiconducting tubes can be excited. From ca. 1.75 eV and below only semiconducting tubes are probed. A corresponding family assignment for selected excitation energies can be seen in Fig. 5.
Fig. 5 Raman spectra of the radial breathing modes (RBM) of the pristine HiPco sample are plotted for several laser excitation energies. SWCNT (2n + m = constant) are denoted that have been determined via pattern recognition.39 |
From the Raman analysis of SWCNT–Phn:1(KCx) we find several statements: (i) after functionalization, the RBM intensities drop notably. Further, our experimental data indicates that a covalent functionalization does not affect the optical transition energies significantly, i.e., for a constant excitation energy we probe the same nanotube types before and after the functionalization. (ii) Carbon nanotubes with smaller diameters are generally more sensitive towards a functionalization compared to those with larger diameters. This can be identified by the significantly stronger depletion of smaller nanotubes' RBMs (higher Raman shifts) in the corresponding Raman spectra (Fig. 6), where the RBM spectra are normalized in intensity to the mode of the nanotube with the largest diameter (smallest Raman shift). This well-known behavior applies for both metallic and semiconducting carbon nanotubes and can be explained by the increased ring strain. (iii) In Fig. 7 Raman spectra are depicted in which both metallic and semiconducting tubes are in resonance. The RBM intensities in the upper part indicate that metallic carbon nanotubes are affected by the functionalization to a larger extent compared to semiconducting tubes. In contrast, the spectra in the lower part (Fig. 7) indicate the opposite behavior, i.e., semiconducting tubes seem to be affected to a larger extent by the functionalization. However, a direct comparison is unfeasible since the effect of a metallicity-selective functionalization is superimposed by the dominant influence of diameter-selective functionalization. To circumvent this aspect, we compare the D-mode intensities where exclusively metallic (2.18 eV) or semiconducting (2.71 eV, 1.68 eV) tubes are in resonance with the laser excitation energy Eexc (see Fig. 8). For Eexc = 2.71 eV (1.68 eV) the tube diameters are larger (smaller) compared to the ones probed for Eexc = 2.18 eV. In all cases we observe an increase of the D-mode intensity after functionalization. However, the intensity increase for metallic carbon nanotubes is larger compared to that of semiconducting tubes with larger diameters and almost equal to smaller semiconducting carbon nanotubes. This direct comparison indicates that the functionalization rather affects metallic carbon nanotubes than semiconducting ones.
As suggested by Laudenbach et al.,56ID/IG values can be utilized to compare the degree of functionalization for different excitation energies. In order to quickly compare the reaction success and to facilitate the determination of nanotube type-dependent selectivity, it is useful to introduce a new term ΔD/G± defined by eqn (2):
(2) |
E exc = 2.71 eV (sc) | E exc = 2.18 eV (m) | E exc = 1.68 eV (sc) | |
---|---|---|---|
SWCNT–Ph(20:1)(KC4) | ΔD/G+: 1.05, ΔD/G−: 1.44 | ΔD/G+: 0.16, ΔD/G−: 1.86 | ΔD/G+: 1.50, ΔD/G−: 1.70 |
SWCNT–Ph(10:1)(KC200) | ΔD/G+: 1.44, ΔD/G−: 2.37 | ΔD/G+: 2.46, ΔD/G−: 2.77 | ΔD/G+: 1.05, ΔD/G−: 1.44 |
Fig. 9 TGA mass loss and ion current traces for reductively arylated sample SWCNT–Ph20:1(KC4) – m/z 78 can be attributed to the protonated detached aryl moieties C6H6˙+ (other fragmentation products are provided in Fig. S13†). |
As outlined above, we have recently found that low potassium charging concentrations (K:C < 1:200) lead to a selective charging of metallic SWCNT helicities.29 Therefore, we wanted to investigate whether this could be utilized in a cooperative manner to increase the amount of selectively functionalized SWCNTs and whether a side product formation could be suppressed by the use of an equimolar amount of trapping reagent to consume the applied negative charges in full extent. Our selection of the reductive conditions is furthermore driven by the results obtained by the DFT calculations, where a supercell consists of several hundred carbon atoms and one single negative charge (see Table 1). The binding energies (Eb) for the diazonium cation with the negatively charged SWCNT species are on average higher for metallic tubes, the maximum differences being about 0.3–0.5 eV. This is the same energy window that has been calculated for the difference of the adsorption energies of potassium atoms on negatively charged metallic SWCNTs in relation to semiconducting species.29 This selective charging of metallic SWCNT species is expected to take place up to a potassium to carbon ratio of 1:200. With this type of charged starting material we should in principle be able to exploit two cumulative selectivity-determining parameters – (a) selective charging of metallic SWCNT helicities and (b) preferred energetic interaction of the diazonium cation with negatively charged metallic SWCNT species. The Raman screening (Fig. 4) of the respective sample (SWCNT–Ph10:1(KC200)) clearly indicates that a reductive arylation under these low charging conditions is possible – obtained ID/IG ratio: 0.39 for Eexc = 2.33 eV (further Raman information is presented in the ESI†). Moreover, the characteristic RBM signature of the carbon nanotubes is also preserved under these conditions, rendering the sample accessible for an in-depth Raman investigation – see below. Regarding the TG-MS characterization data, SWCNT–Ph(10:1)(KC200) exhibits a total mass loss of around 15.7% (Fig. 10). Here, the characteristic masses of the bound benzene moiety (m/z 78, C6H6.+; m/z 77, C6H5+; m/z 51, C4H3+) can be detected as main peaks at around 310 °C, which, as outlined above, is the typical temperature regime for the cleaving of covalently attached aryl addends. In addition, SWCNT–Ph(10:1)(KC200) shows only minor framework degradation as opposed to the reductively arylated sample with a sub-equimolar concentration of the diazonium cation SWCNT–Ph20:1(KC4). Therefore, it can be concluded that under the chosen conditions the reductive arylation of the carbon nanotubide intermediates proceeds in a clean fashion, hinting that the calculated DoF of 1.2% is a good approximation, unlike for sample SWCNT–Ph(20:1)(KC4). This is also consistent with a higher ID/IG ratio in the Raman spectra (Fig. 4).
These findings are further corroborated by a gas chromatographic separation and characterization of the thermally detached gaseous components. In Fig. 11 the respective GC elugrams of SWCNT–Ph10:1(KC200) and SWCNT–Ph20:1(KC4) are compared. For SWCNT–Ph(10:1)(KC200) the elugram clearly shows benzene as only analyte peak at an injection temperature of 280 °C. Biphenyl or longer polyphenyl chains obtained by a radical recombination of the intermediately generated aryl radicals were not detected. For SWCNT–Ph(20:1)(KC4), only a minor fraction of detached benzene can be found at an injection temperature of 280 °C (Fig. 11 – red trace). Furthermore, at an injection temperature of 480 °C, several aromatic components like toluene, indicative for a SWCNT framework decomposition,57,58 can be detected for SWCNT–Ph(20:1)(KC4) (Fig. S14†). These results clearly underline that SWCNT–Ph(10:1)(KC200) represents an appropriate sidewall-functionalized SWCNT sample and is suitable for analysis of the underlying electronic type selectivity by means of resonance profile analysis of the Raman RBM region. Fig. 8 and Table 4 enable to directly compare the ID/IG ratios of the two systems SWCNT–Ph20:1(KC4) and SWCNT–Ph10:1(KC200). It can be seen that the ID/IG ratios for SWCNT–Ph10:1(KC200) are larger for all laser excitation energies, probed both for metallic and semiconducting carbon nanotubes, indicating that the SWCNT–Ph10:1(KC200) functionalization is more efficient compared to the SWCNT–Ph20:1(KC4). This is in accordance with TG-MS results and nicely confirms our rationale that the two electronic type determining parameters can be used in a cooperative fashion.
On the basis of our results the underlying parameters for a selective functionalization of metallic SWCNTs with diazonium cations could be elucidated. In ongoing studies, the DFT approach can now be extended to further trapping electrophiles, like alkyl and aryl halides and λ3-iodanes.
Footnotes |
† Electronic supplementary information (ESI) available: Experimental details regarding the reductive charging of HiPco SWCNTs and additional Raman and TGA analysis. In addition, theoretical details regarding the structural parameters, the calculated structures of the SWCNT/diazonium interaction, and the electronic properties of the studied system. See DOI: 10.1039/c8sc03737j |
‡ Both authors contributed equally to the present study. |
This journal is © The Royal Society of Chemistry 2019 |