aInstitute of Electrical Engineering, Slovak Academy of Sciences, Bratislava, Slovakia. E-mail: prerna.chauhan@savba.sk
bSlovak University of Technology, Univ. Sci. Park Bratislava Centre, Vazovova 5, 812 43 Bratislava, Slovakia
cInstitute of Physics, Slovak Academy of Sciences, Bratislava, Slovakia
dJoint Institute for Nuclear Research, Dubna, Russia
eCenter for Device Thermography and Reliability, University of Bristol, Bristol BS8 1TL, UK
fInternational Laser Centre, Ilkovičova 3, Bratislava, Slovakia
First published on 26th November 2019
Thick InAlN layers (In-molar fraction >0.37) on GaN buffer layers were prepared using a close-coupled showerhead metalorganic chemical vapor deposition (MOCVD) reactor. This work provides a discussion of the dependence of reactor parameters (pressure, ammonia flow and temperature) and unintentional Ga-incorporation on structural, optical and chemical properties of those layers down to the nanoscale. Rutherford back-scattering spectrometry, Auger electron spectroscopy, and transmission electron microscopy with the energy dispersive X-ray analysis were used for in-depth chemical analysis of layers. A diminishing Ga-auto-incorporation in thick InAlN layer creates a chemically graded InAl(Ga)N interlayer that assists in releasing of interfacial strain and paves the way toward In-rich InAlN layer. The rate of unintentional Ga-auto-incorporation in InAlN layers increases with decreasing of growth temperature, and increasing of reactor pressure and ammonia flow during growth. Raman and photoluminescence spectroscopy were used to get the crystal structural fingerprint influenced by Ga-incorporation. We suggested that Ga could incorporate at nitrogen vacancies at high reactor pressures (≥200 mbar). Screw dislocations and/or N-vacancies in InAl(Ga)N layers may be energetically favorable sites for In-incorporation and lead to compositional fluctuation and local In-rich InAl(Ga)N phase.
MOCVD growth of In-rich InAlN is very challenging due to the very different optimal growth conditions of binaries InN, GaN and AlN. Reuters et al.3 have also proposed a virtual multi-layer model to describe relaxation and In-incorporation in thin (52–75 nm) InAl(Ga)N layers in the direction of growth by means of Rutherford backscattering spectrometry (RBS) and high-resolution X-ray diffraction (HR-XRD). Precise control of the elemental molar fraction and their in-depth distribution is crucial to ensure desired optical and electronic properties of InAlN layers.
In our previous work,1 we demonstrated that diminishing Ga depth profile in InAl(Ga)N layer growth is helping in strain relaxation, which further assists in In-incorporation. We observed that under N2 carrier gas, the unintentionally incorporated Ga create an InAl(Ga)N layer at the interface with GaN buffer. In subsequent layer growth, a graded InAl(Ga)N layer accompanied by strain relaxation to reach InAlN with Ga ∼ 0 was formed. A crucial parameter for InAl(Ga)N growth is ammonia (NH3) flow to supply sufficient N content to avoid features formed in InAl(Ga)N due to N deficiency, like pits with N vacancies and In droplets. NH3 decomposition efficiency is low at growth temperature ∼700 °C, so high partial pressure of NH3 is highly recommended. In MOCVD, the high partial pressure of any element can be achieved by either high reactor pressure or high flow. High reactor pressure promotes the reaction between trimethylaluminum (TMAl) and NH3 that leads to the enhanced adducts formation.9,10 Consequently, less Al-containing moieties would be available for taking part in InAl(Ga)N layer formation on the substrate surface and all together limit the growth rate. The high NH3 partial pressure generates a high amount of H2 molecules, which reduces In droplets on InAl(Ga)N surface but at the same time reduces In-incorporation and enhances pit density. Similar observations were reported earlier.9–11
In the present work, the influence of growth parameters on depth-profile of Ga-auto-incorporation is discussed in detail. Up to now, defects evolution and characteristics of dislocations associated with InAlN layers have been investigated microscopically by transmission electron microscopy (TEM).6–8 However, for InAl(Ga)N layers such investigations are still missing and we contribute to fill this gap. To validate the In-molar fraction and Ga-auto-incorporation due to the memory effect, the samples were analyzed by RBS, Auger electron spectroscopy (AES) and TEM with the energy dispersive X-ray (EDX) analysis that provide complementary insights by probing the chemical composition depth-profile, layer quality and defects along the growth direction.
Samples | T (°C) | Carrier gas | P (mbar) | Q vol NH3 (sccm) | V/III ratio | t (nm) | In m.f. XRD | InAl(Ga)N | AFM RMS (nm) | |
---|---|---|---|---|---|---|---|---|---|---|
ω 0002 (°) FWHM | ω 101 (°) FWHM | |||||||||
S1 (ref. 1) | 790 | H2 | 70 | 1500 | 5087 | 165 | 0.09/0.12 | 0.20 | 0.60 | 3.1 |
S2 (ref. 1) | 775 | H2 | 70 | 1500 | 5087 | 171 | 0.11/0.13 | 0.22 | 0.62 | 8.9 |
S3 (ref. 1) | 760 | H2 | 70 | 1500 | 5087 | 210 | 0.15 | 0.17 | 0.32 | 9.5 |
S4 (ref. 1) | 730 | H2 | 70 | 1500 | 5087 | 220 | 0.18 | 0.12 | 0.40 | 30.6 |
S5 (ref. 1) | 730 | N2 | 70 | 1500 | 5087 | 285 | 0.37 | 0.66 | 1.6 | 3.8 |
S6 | 730 | N2 | 70 | 2000 | 6783 | 300 | 0.36 | 0.51 | 1.4 | 9.5 |
S7 | 730 | N2 | 70 | 2500 | 8478 | 296 | 0.35 | 0.53 | 1.2 | 8 |
S8 | 730 | N2 | 70 | 3000 | 10174 | 300 | 0.36 | 0.54 | 1.2 | 6 |
S9 | 730 | N2 | 100 | 1500 | 5087 | 260 | 0.37 | 0.77 | 1.4 | 4.3 |
S10 | 730 | N2 | 150 | 1500 | 5087 | 316 | 0.37 | 0.54 | 1.4 | 6.8 |
S11 | 730 | N2 | 200 | 1500 | 5087 | 283 | 0.38 | 0.73 | 1.8 | 8 |
S12 | 730 | N2 | 200 | 3000 | 10174 | 274 | 0.41 | 0.83 | 1.4 | 10.5 |
S13 | 730 | N2 | 200 | 4500 | 15261 | 235 | 0.38 | 0.83 | 1.5 | 16 |
S14 | 730 | N2 | 250 | 3000 | 10174 | 215 | 0.41 | 0.76 | 1.4 | 15 |
S15 | 730 | N2 | 250 | 4500 | 15261 | 117 | 0.40 | 0.70 | 1.4 | 10 |
S16 | 730 | N2 | 300 | 3000 | 10174 | 224 | 0.42 | 0.73 | 1.5 | 27.5 |
S17 | 730 | N2 | 300 | 4500 | 15261 | 160 | 0.43 | 0.52 | 1.5 | 30.7 |
S18 | 730 | N2 | 350 | 3000 | 10174 | 178 | 0.44 | 0.53 | 1.8 | 13 |
S19 | 730 | N2 | 400 | 3000 | 10174 | 111 | 0.47 | 0.36 | 1.5 | 16.8 |
S20 | 730 | N2 | 400 | 3500 | 11869 | 120 | 0.46 | 0.38 | 1.3 | 21.7 |
S21 (ref. 13) | 730 | N2 | 400 | 4500 | 15261 | 112 | 0.47 | 0.49 | 1.1 | 7.8 |
For all samples, XRD 2θ/ω 0002 and 101 scans were carried out on Bruker D8 DISCOVER diffractometer to evaluate the crystalline quality and approximate In-molar fraction.12 Atomic force microscopy (AFM) (NTEGRA Prima, in tapping-mode) and scanning electron microscope (SEM) (FEI Quanta 250 FEG) were used to characterize the surface morphology. LayTec EpiCurve® TT in situ monitoring system was used to extract growth rate (Rg) and the thickness (t) of InAl(Ga)N layers with pyrometer reflectance at 632.7 nm. Cross-sectional SEM was used to verify the thickness of InAl(Ga)N layers with an approximate 5% error as estimated by in situ reflectance curves. Absorption (UV-VIS-NIR Spectrophotometer SolidSpec-3700) and photoluminescence (PL, OLYMPUS BX51 microscope with He-Cd laser 325 nm) measurements were done to characterize the InAl(Ga)N layers grown under different conditions. For Raman spectroscopy, Renishaw InVia™ spectrometer in backscattering geometry was used with a 488 nm excitation laser wavelength. To check the In-molar fraction and Ga-auto-incorporation due to the memory effect, selected samples were investigated by Auger depth profiling (JEOL JAMP 9510-F Auger microprobe, using 10 keV electron excitation with 10 nA beam current, 55° tilt with respect to primary electron beam, normal take-off angle), Rutherford backscattering spectrometry (RBS) and high-resolution transmission electron microscopy (HRTEM). Polarity was determined by using convergent beam electron diffraction (CBED) patterns along the [100] zone axis of GaN buffer, as we did not detect any inversion domain at the InAl(Ga)N/GaN interface, we can state that the samples investigated here are In-polar grown on Ga-polar GaN buffer layer. High-angle annular dark-field (HAADF) and bright-field (BF) images were taken to evaluate the chemical contrast together with EDX analysis using an aberration-corrected FEI Titan Themis 300 microscope in STEM mode. The microscope was operated at 200 kV acceleration voltage and EDX acquisition was carried out using a Super-X detector system (ChemiSTEM technology).
With the pressure above 200 mbar for a constant NH3 flow, FWHM of the 0002 diffraction peak of InAl(Ga)N decreased rapidly (shown in Table 1). In our opinion, the effect could be due to improved InN bonding and negligible In-segregation at higher pressure, the otherwise high vapor pressure of N2 over InN leads to the In-segregation and hampers the growth of In-rich InAl(Ga)N. Accompanying the decrement of 0002 FWHM, the FWHM of 101 was almost constant. These values of 0002 and 101 FWHM can be used to estimate the screw and edge threading dislocation densities according to1
(1) |
Distinct curves reflectivity in regions (iii) and (iv) with increasing reactor pressure demonstrate the different interface and InAl(Ga)N layer properties, respectively. The reflectance is a function of the surface roughness and refractive index, which depends on the chemical composition of the material. At the end of region (iii), reflectance increased with pressure. At the used pyrometer wavelength (632.7 nm), the trend in the refractive index of binaries is InN > GaN > AlN.16 Therefore, we believe that the increased Al content at the interface could be a possible reason for the increased interface roughness due to the low surface mobility of Al. Consequently, the low refractive index leads to the lower observed reflectance at 70 mbar. With increasing reactor pressure, more incorporation of In and/or Ga influence reflectance. With increasing reactor pressure, the growth rate and consequently, the thickness of InAl(Ga)N layers decreases. The approximate thicknesses of InAl(Ga)N layers are presented in Table 1. This decreasing thickness trend corroborates the loss of precursors in the form of gas-phase parasitic reactions and formation of adducts as shown in Fig. 2.
PL and absorption spectra of the samples obtained at room temperature are shown in Fig. 4(a) and (b), respectively. With the increase of pressure from 70 mbar to 200 mbar, the red-shifted PL peak accompanies the reduced PL intensity. This indicates, that besides the edge dislocation some other factor is also contributing, that causes PL peak shift and related to reactor pressure, unlike ref. 1. For GaN, the absorption edge (AE) was determined by extrapolating the linear region to the baseline, as shown by the dashed line in Fig. 4(b). All samples exhibit distinct GaN AE around 3.42 eV, which is consistent with the measured GaN near band edge (NBE) peak in Fig. 4(a). In PL measurements, inhomogeneities due to compositional fluctuations often lead to the broadening of the emission band. A good example of the broadening is given in ref. 17, where calculations confirm that the alloy fluctuations in InGaN QWs are responsible for the broadening of PL when compared with a QW system without alloy in the active region. It is difficult to determine whether the compositional fluctuation is the dominant effect or if a different mechanism contributes to the broadening of the PL peaks. Toward the low energy side with a reference to the sharp GaN AE, all samples have a broad absorption knee or slowly decreasing absorption up to ∼1.90 eV.
As the GaN lies underneath InAl(Ga)N, one would expect most of the light with the photon energy above the bandgap to be absorbed in the InAl(Ga)N, and therefore, the GaN absorption edge would be indiscernible. Since this is not the case, we would surmise that the absorption in the InAl(Ga)N is relatively weak as shown in Fig. 4(b). The broad absorption knees and the substantial change in their shape with the change of reactor pressure confirm a direct absorption in the InAl(Ga)N layers. The absorption is either influenced by the compositional gradient or defects in InAl(Ga)N layers. For quaternary InAl(Ga)N or lnxAlyGa1−x−yN relationship between the chemical composition and bandgap (Eg) is usually stated by utilizing the Vegard's law:1
Eg(x) = xEg(lnN) + yEg(AlN) + (1 − x − y)Eg(GaN) | (2) |
To gain more insight, the PL and absorption spectra of selected samples are presented in Fig. 5. At 70 mbar, a broad and asymmetric PL peak centered around 2.45 eV with a shoulder at the high-energy side ∼2.96 eV was observed. The deconvolution analysis provides three distinct Gaussian peaks centered around 2.96, 2.45 and 2.12 eV; we assume that these three peaks correspond to the near band edge (NBE), blue luminescence (BL) and yellow luminescence (YL), respectively. In MOVCD growth, carbon (C)-incorporation is higher at the low reactor pressure and C at nitrogen site (CN) and C at interstitial sites (Ci) could be the most probable reason behind BL band transitions.18
In our previously reported sample grown at 70 mbar pressure and 1500 sccm NH3 flow,1 we attributed YL band to the transition from shallow donors, V+N and O+N, to deep acceptors, group-III cations vacancies V3−III and their complexes V3−III − O+N, V3−III − (O+N)2.1 The same attribution will continue for YL of sample grown at 70 mbar pressure and 3000 sccm NH3 flow. However, V3−III may fill up as pressure increased. This is confirmed by the disappearance of YL band and appearance of red luminescence (RL) band at higher pressures, 200 and 400 mbar. At 200 and 400 mbar, the PL peaks are observed at 1.94 eV with FWHM of 8.2 eV and at 1.86 eV with FWHM of 7.9 eV, respectively, which is coinciding with their absorption onset (marked by orange arrow). This 80 meV red-shifted PL peak is accompanied by 94% decreased intensity. Moreover, their tail extends toward the high-energy side. This validates the defect-related radiative recombination and most likely due to the Ga at nitrogen site (GaN).19 Such non-radiative defects quench PL. This suggests the freezing of free carriers from the conduction band occurred at 200 mbar due to trapping at the deep acceptor energy levels.
The broad RL band may be the result of strong electron–phonon interaction due to the recombination of carriers at the deep acceptor level. Electron–hole recombination is accompanied by non-radiative phonon transitions, which we acquired using Raman spectroscopy shown in Fig. 6. High spatial order and long-range translational symmetry in high crystal quality binary semiconductors (such as GaN buffer layer) result in narrow Raman peaks. Alloying of additional elements resulting in ternary and quaternary crystals create spatial disorder responsible for broadening of Raman peaks as observed in studied InAl(Ga)N layers. Table 2 summarizes the InAl(Ga)N Raman phonon modes frequencies and shift with reference to Kang et al.20 Red-shifted E2(TO) mode indicates the increased tensile stress in this layer. We assume this could be due to the presence of Ga in InAlN lattice. The localized wave function of a hole at GaN distorts the atomic symmetry and crystal structure expands outward, as illustrated in Fig. 7. Consequently, A1(LO) polar phonon modes are influenced due to the modified intrinsic electric field.21
InAl(Ga)N Raman phonon modes | Kang et al.20 | This work | ||
---|---|---|---|---|
Estimated values for 0.41 In mf (cm−1) | Estimated values for 0.47 In mf (cm−1) | 0.41 In mf/XRD at 200 mbar (cm−1) | 0.47 In mf/XRD at 400 mbar (cm−1) | |
E2(TO) | 565.6 | 556.3 | 547 (−18.6) | 548 (−8.3) |
InN-like A1(LO) | 663.2 | 655.0 | 672 (+8.8) | 669 (+14) |
AlN-like A1(LO) | 771.0 | 755.5 | 758 (−13) | 751 (−4.5) |
Fig. 11 RBS depth profile of InAl(Ga)N layers grown at 70 mbar pressure and 1500 sccm NH3 flow.1 The directed black arrows are guide to the eye and show the influence of decreasing temperature (790 to 730 °C) and carrier gas (H2 to N2 at 730 °C) on depth profile of In-, Al- and Ga-molar fraction. |
Fig. 11 illustrates that the decreasing growth temperature from 790 to 730 °C results in a much higher increase in In-molar fraction than Ga-molar fraction. Moreover, with decreasing growth temperature, the growth rate increases, accompanied by increasing Ga-incorporation and decreasing Al-molar fraction. This indicates that Ga replaces Al. However, the growth rate increases to maintain the total amount of Al during deposition. InAl(Ga)N layers are Ga-rich at the interface and with the progression of the growth, layers became Al- rich at the surface. In the InAl(Ga)N layer grown with N2 carrier gas at 730 °C Ga-incorporation decreased. A quaternary InAl(Ga)N layer with ∼50 nm thickness was formed unintentionally at the interface, with Ga decreasing (from 0.19 to 0.01), In increasing (from 0.28 to 0.37) and Al increasing (from 0.54 to 0.62) toward the surface. On the other hand, the subsequent rest of the layer is almost ternary In0.37Al0.63N. This Ga-gradient is much smaller than in the layer grown with H2 carrier gas at 730 °C and at the interface, Ga-incorporation decreased by 72% and Al-incorporation increased by 100% when compared with H2 carrier gas.
Fig. 12 AES depth profile of InAl(Ga)N/GaN HSs. InAl(Ga)N layers are grown at different pressures (70 and 200 mbar) and different NH3 flow (1500 and 3000 sccm) under N2 carrier gas at 730 °C. APPH fraction is defined in ref. 1. Blue color marked the signals from GaN buffer. |
The layers grown at 200 mbar, but with 1500 and 3000 sccm NH3 flow include quaternary In0.26Al0.43Ga0.31N and In0.26Al0.46Ga0.34N near GaN buffer, respectively; and In0.42Al0.48Ga0.05N and In0.42Al0.5Ga0.05N located approx. 30 nm below the surface, respectively. At the 3000 sccm NH3 flow, the thickness of InAl(Ga)N layer is 50 nm less and has relatively more Ga- and Al-incorporation. The reduced growth rate could be attributed to the higher Al content as observed in RBS. We conclude that Ga-incorporation increases with increasing reactor pressure. This trend is consistent with the previous report,13 where InAl(Ga)N layer grown at 400 mbar and 4500 sccm NH3 flow was observed with a higher Ga-incorporation. Naturally, thicker InAl(Ga)N layers have a less Ga on top.
The higher NH3 flow produces higher H content, which was confirmed by elastic recoil detection analysis (ERDA). At 200 mbar, the InAl(Ga)N layer grown with 3000 sccm NH3 flow has 3.5% H, while the InAl(Ga)N layer grown with 1500 sccm NH3 flow has only 1%. Increased H or reduced N vacancies could be the possible cause of the reduced free carrier concentration, which is corroborated by the missing blue luminescence (BL) in PL spectra in Fig. 4. This could be attributed to the reactive behavior of H that reduces impurities and passivates the donors (N vacancies). In Fig. 12, variation in O depth profile indicates that either the source of O impurity is NH3 or the surface roughness makes it more exposed to the environmental O, and consequently, more oxidized.23 In the same figure, C is attributed to surface contamination.
To go deeper into details about the influence of reactor pressure and NH3 flow on the growth evolution at nano-level, the layer cross-sections and chemical elements distributions are investigated. Fig. 13 shows the cross-sectional HAADF and BF images along with the corresponding EDX maps for a InAl(Ga)N layer grown at 70 mbar pressure and 1500 sccm NH3 flow (also analyzed in Fig. 11 and 12 by RBS and AES, respectively). The interface layer is quaternary and homogeneous, while the subsequent InAlN layer with 0.37 In-molar fraction exhibits inhomogeneous regions with dark contrast vertical line (In-poor) and void in V-shaped pits, which all together leads to a saw-tooth surface morphology. The quaternary layer appears to have a better crystalline quality possibly due to the presence of Ga, which might enhance miscibility and consequently, suppress phase separation in InAl(Ga)N. A similar cross-section view and features were observed for 500 nm thick InAlN lattice matched to GaN.24
The surface roughness sensitivity of RBS technique and high channeling due to In-incorporation at preferential sites or random compositional fluctuations at high-pressure growth may underestimate the chemical molar fraction. Due to the limited depth resolution of RBS technique (channel length ∼30 nm), it is difficult to comment on the exact limit where the relaxation takes place in the layer. Hence, for layers grown at ≥200 mbar pressure, the most reliable chemical data could be obtained by the EDX. The HAADF image with EDX analysis reveals that strain relaxation or In-incorporation mechanism is entirely different for layer grown at 200 mbar pressure (shown in Fig. 14). Homogeneous InAl(Ga)N interlayer accommodating strain is also observed, which upon relaxation turned to inhomogeneous. This indicates that the increase in In-incorporation is associated with the strain relaxation in InAl(Ga)N layer, which is consistent with the previous findings.1,2,25,26 At the InAl(Ga)N layer/GaN interface, graded layers allow strain-driven In-incorporation. However, strain relaxation via pit formation due to low surface mobility of Al-adatoms provides favorable incorporation sites for In-adatoms and locally In-molar fraction reaches up to 0.51. Higher growth rate and hence, more compositional fluctuation associated with screw dislocations and/or N-vacancies was observed at 200 mbar in comparison to the layer grown at 400 mbar with a lower growth rate. The EDX data is in good agreement with the chemical trend observed in the absorption spectra, AES and RBS data. This varying chemical depth profile in InAl(Ga)N layer explains the observed broad absorption knee. Reflection at the InAl(Ga)N/GaN interface is also influenced by chemical composition. Furthermore, the growth mechanism changes with the growth pressure and is discussed in the next section.
Different growth kinetics, local lattice dynamics and growth evolution are demonstrated in Fig. 13 and 14 for InAl(Ga)N layers grown at 70 and 200 mbar reactor pressures, respectively. On that basis, in the following, we will demonstrate the growth mechanism of the InAl(Ga)N layers illustrated in Fig. 15. At low growth pressure, the enhanced surface mobility of Al and poor incorporation efficiency of In form Al-rich InAl(Ga)N layer at the interface. Up-on subsequent layer growth, In replaces Ga and generated compressive strain is released via pits, which are the preferential incorporation sited for In-adatoms and as a result, hillocks occur. For the layer grown at 200 mbar, the pressure enhances In- and Ga-incorporation and the diminishing profile of Ga is benefitted to both In and Al. At this pressure, grains with different In-molar fraction lead to the formation of smaller and denser hillocks. At 400 mbar pressure,13 Al- and/or Ga-rich grains are also formed due to their parasitic reactions and low surface mobility and distributed all over the layer along with the smaller and denser hillocks. In-compositional instability induced by the two thermodynamics factors, i.e. growth temperature, and pressure, is the combined effect of strain and incorporation sites like pits, screw dislocations and rough surface. These sites are generated during the layer growth itself either by higher growth rate or strain relaxation.
Higher pressure is favorable for reducing N vacancies that lead to decreased carrier concentration and photoluminescence. An interesting measurement to investigate this further would be to study the temperature dependence of the PL. At the low temperatures, if the interpretation is correct, the photogenerated carriers may be trapped by the defects in GaN, so we might expect to see the emission from GaN, and less intense emission from the InAl(Ga)N layer.
This journal is © The Royal Society of Chemistry 2020 |