Zirconium-based coatings exhibit a range of useful properties such as high hardness, high temperature stability, biocompatibility, and good resistance to wear, erosion, corrosion and oxidation, making them suitable candidates for use in tribological, biomedical, corrosion-resistant, nuclear fuel, electrical and decorative applications. Common deposition methods reported for Zr-based coatings include cathodic vapor deposition, plasma enhanced chemical vapor deposition, magnetron sputtering, reactive sputtering, reactive melt infiltration, laser pulse deposition, etc. Both single and multilayered coatings are produced. This paper presents a review of the effects of deposition methods and operational conditions on the properties of zirconium carbide, zirconium nitride and zirconium carbonitride hard coatings. It describes the role of various process parameters used during the deposition of advanced functional coatings. The present study will contribute to the understanding of hard coatings in general.
Clifton and Johnson2 patented a method for preparing ZrC fibers in 1968 by reacting carbon with Zr-oxide fibers. The developed product had a higher melting temperature compared to the zirconium oxide fibers in use at the time. ZrC fibers exhibited lower thermal conductivity and were stable within the operational temperature range. The application of ZrC as a coating on carbon fibers was first reported by Killin et al. in 1975.3 His group evaluated the oxidation resistance of ZrC-coated carbon fibers. In the same year, tungsten fibers were coated with ZrC using a flow-type quartz reactor by Samoilenko and Pereselentseva.4 Such fibers were used as reinforcement in metal matrix composites such as Ni- and Co-based alloys.
Another novel application reported by Reynolds et al. in 1975–1976 consisted of vapor deposition of ZrC coatings on fuel particles to improve the latter's irradiation behavior in a high temperature gas-cooled nuclear reactor.5,6 It was observed that the coatings successfully retained the fission products. ZrC was selected due to its high melting temperature, reduced tendency to form low-melting-point phases and relatively low neutron-absorption cross-section. ZrC exhibits higher temperature stability than SiC-coated tri-structural isotropic (TRISO) fuel particles. After Reynolds’ initial work, research groups in Japan have worked towards developing this technology further in the subsequent decades.7–14 In addition, contributions to this field from researchers working in the United States,15–17 France18 and China19–22 are also reported in the literature.
In the 1990s, coatings of Ti-based carbides and nitrides were increasingly being used to protect cutting tools. Although similar studies on ZrC were comparatively limited, its characteristics such as high melting temperature, hardness, and corrosion and wear resistance established it as a potential candidate for use in tribological applications. In 1993, reactive magnetron sputtered ZrC coatings with high concentrations of carbon were reported to exhibit hardness values as high as 5000 HV.23 Vacuum plasma sprayed coatings exhibited 1600 HV microhardness.24 Various studies that evaluated the tribological properties of ZrC form part of the related literature.25–29
A ZrC coating was identified as a potential candidate to protect components in high temperature environments.30 Due to its low work function (3.5 eV), it was used as a coating on field emitters to improve the emission stability of field emission scanning electron microscopes.31 ZrC was successfully coated on roller contacts using a physical vapor deposition technique in 2004.32 A hardness and a Young's modulus of 1500 HV and 200 GPa were recorded for these coatings. ZrC coatings were also employed in rolling contacts due to their high slip-rolling resistance.33 ZrC coatings were also evaluated for biomedical applications such as in improving the corrosion resistance and hemocompatibility of implant materials, e.g., SS316L34 and Ti.35 They were also used to improve the biological safety of biomedical NiTi shape memory alloys.36,37 Due to its high electrical conductivity and chemical inertness, potential use of ZrC in sliding electrical contacts such as brushes, microelectromechanical devices, circuit breakers and motor vehicle starters has been suggested.38
Various synthesis methods reported for ZrC include cathodic vapor deposition (CVD),39 magnetron sputtering,40 reactive melt infiltration,41 reactive sputtering42 and PECVD-PIP.43 Laser pulse deposition has also been employed to produce single-layered ZrC44,45 and multilayered ZrC/TiN46 and ZrC/ZrN47 coatings with reported hardnesses of above 40 GPa.
The potential of sintered ZrN materials for use in machine tools had been recognized from 1960 through the 1970s.48–51 Zabolotskii et al. coated carbon fibers with ZrN in 1977.52 Zirconium nitride was studied as a metal coating in 1977 by Caillet et al.53 In this study, the oxidation kinetics of the coating was determined. Sputtered ZrN was identified as a wear resistant coating material for tribological applications as well as a barrier material for integrated circuit processing in the early 1980s.54–58 Derradji and Kassabji used a plasma spray method to produce ZrN coatings for possible use in tool applications in 1986.59 Valikhani and Chandrashekhar60 compared the performances of twist drills coated with ZrN and TiN in 1987 with the conclusion that the ZrN outperformed the TiN in terms of service lifetime and the quality of drilling. The erosion behavior of ZrN coatings was studied by Sue et al. in 198861 and 1990.62 Various studies were conducted on ZrN coatings in the following two decades to evaluate their erosion protection for turbine and compressor blades,63,64 microhardness,65–67 adhesion,65 wear at 500–600 °C,68 biocompatibility,69 orientation dependence,70 optical and electrical properties,71 tribology,72 nuclear fuel element compatibility,73 and composition and bonding.74
From 2011 onwards, investigation into Zr-nitride has continued with various aspects under study including hardness, orientation and phase transition,75 erosion,76 microstructure and corrosion,77 tribology,78 the colors of coatings,79 the influence of synthesis parameters,80–82 adhesion and wear,83 the influence of yttrium on microstructure and mechanical properties,84 diffusion barrier properties for nuclear fuel applications,85,86 the bio- and cyto-compatibility of human body implants,87–92 optical, electrical and electronic properties,93–96 oxidation97 and modeling and computational analysis.98–100
Use of Zr-carbonitride as a coating was first reported by Sintsova and Kbzlovskii in 1970.101 It was stated that a Zr-carbonitride coating served to increase the corrosion resistance of a steel substrate while retaining the latter's strength. In 1978, Caillet et al. studied the oxidation kinetics of Zr deposited with Zr-carbonitride coatings.102 Berndt et al. used a CVD technique to synthesize Zr-carbonitride films in 1995 and study their composition, crystallinity and morphology.103 Manier et al. evaluated Zr-carbonitride coatings for slip rolling resistance in 2010.33 Various investigations on Zr-carbonitride coatings were undertaken in recent years to study their synthesis parameters,104 characterization,105 and optical106 and biomedical applications.107–114
This study presents a review of zirconium carbide, zirconium nitride and zirconium carbonitride hard coatings used for various applications. This paper highlights various methods used for the deposition of these coatings and describes the effects of synthesis parameters on the structure and quality of coatings. The words ‘coating’ and ‘film’ are used interchangeably in this paper.
Amongst the reported studies on ion beam deposition methods for ZrC, ZrN and ZrCN coatings are the effect of the methane (CH4) flow ratio on the micro-nano-structure and hardness of carbo-nitride coatings deposited on AISI 304 stainless steel,121 ZrCN coatings deposited by a duplex process that combines ion implantation and magnetron sputtering,104 and epitaxial growth of ZrN/W multilayers using the dual ion beam sputtering (DIBS) deposition method on MgO(001) substrates with bilayer periods of 2.5 nm to 50 nm.122
S/N | Ref. | Coating composition | Method of deposition | Properties | |||||
---|---|---|---|---|---|---|---|---|---|
Hardness | Wear resistance | Corrosion resistance | Friction coefficient | Behaviour with water | Modulus of elasticity | ||||
1 | Shao-Long et al.134 | ZrC | Low pressure chemical vapour deposition (CVD) | Mass and linear ablation rates: 0.86–1.1 × 10−4 g s−1 and 0.23–0.47 × 10−3 mm s−1, respectively | |||||
2 | Ying Long et al.130 | ZrC and ZrC0.85 | Chemical vapour deposition (CVD) | ZrC: 24–26.6 GPa, ZrC0.85: 21.5–24.1 GPa | ZrC: 303–321 GPa, ZrC0.85: 291–313 GPa | ||||
3 | M. Braic et al.128 | TiN/ZrN and ZrN/TiN | Deposition by reactive pulsed magnetron sputtering (RPMS) and radiofrequency beam assisted pulsed laser deposition (RF-PLD) on Si and high speed steel | Vickers micro-hardness (HV0.005): RM coatings – TiN: 24 GPa, ZrN: 21 GPa, TiZrN: 28 GPa, TiN/ZrN (200/32): 32 GPa, ZrN/TiN (200/32): 30 GPa, ZrN/TiN (10/50): 14 GPa; PL coatings – ZrN/TiN (10/50): 6 GPa | |||||
4 | Siao-Fan et al.125 | CrN/ZrN multilayer coatings | Deposited using a cathodic arc system | Average monolayer coating hardness CrN: 20.3 GPa, ZrN: 21.9 GPa; the maximum multilayer coating hardness (about 28.8 GPa) was achieved with a Cr/Zr atomic ratio of 2.7 | Average monolayer coating modulus of elasticity CrN: 228 GPa, ZrN: 267 GPa; the maximum multilayer modulus of elasticity (about 276 GPa) was achieved with a Cr/Zr atomic ratio of 2.7 | ||||
5 | E. Silva et al.117 | ZrCN | DC reactive magnetron sputtering | 10.6–32.4 GPa | Wear rate: 0.38 ± 0.97 to 2.27 ± 0.25 m3 N−1 Lap−1 × 1015 | 173.7–326.9 GPa | |||
6 | K. T. Rie and J. Whole132 | ZrCN | Pulsed DC PACVD technique; below 200 °C | 1400 HK0.01 | |||||
7 | V. Braic et al.135 | (Zr, Ti)CN coatings | Magnetron sputtering | 25–29 GPa | More electropositive than an uncoated Ti6Al4V substrate and ZrCN | Hydrophobic; contact angle, 100° | |||
8 | M. Braic et al.123 | ZrCN and multi-layered Zr/ZrCN | Cathodic method with C45 and M2 steels as substrates | ZrCN: 19.5–28 GPa, Zr/ZrCN: 10.4–21.4 GPa | Scratch test adhesion critical load: ZrCN: 44–54 N, Zr/ZrCN: 74–43 N | ||||
9 | M. M. Larijani et al.121 | ZrN1−XCX where 0 ≤ X ≤ 1 | Deposition by an ion beam sputtering method on AISI 304 stainless steel at 400 °C | The maximum hardness was 2520 HV for x = 0.57 | |||||
10 | E. Grigore et al.104 | ZrCN | Duplex process that combines ion implantation and magnetron sputtering | The range of the micro-hardness of the coatings obtained was 3180 to 4050 HV0.05. The highest value obtained was with a C/N atomic ratio of 0.9 | The highest value of micro-hardness was obtained with a C/N atomic ratio of 0.9 while it exhibited the poorest wear resistance | ||||
11 | M. Braic et al.118 | (Zr,Nb)CN, (Zr,Ti)CN and (Zr,Hf)CN | Reactive magnetron sputtering technique | ZrCN: 21.4 GPa & 23.6 GPa, (Zr,Nb)CN: 23.1 GPa & 25.4 GPa, (Zr,Ti)CN: 21.4 GPa & 24 GPa and (Zr,Hf)CN: 25.1 GPa & 29.3 GPa | ZrCN: 0.32 & 0.3, (Zr,Nb)CN: 0.32 & 0.27, (Zr,Ti)CN: 0.38 & 0.28, and (Zr,Hf)CN: 0.51 & 0.24 | ||||
12 | P. Dubey et al.116 | Zirconium tungsten nitride (ZrXW1−XNY) | Reactive magnetron sputtering technique | The dual phase (fcc + hcp) film showed maximum hardness (∼24 GPa) | The single phase (fcc) film showed maximum (H/Er2 ∼0.2 GPa) and fatigue fracture (H3/Er2 ∼0.87 GPa) | The dual phase (fcc + hcp) film showed a maximum reduced modulus of elasticity (135 GPa) |
Due to lateral variation in plasma energies, the pulse laser deposition technique gives rise to changes in layer thickness across the sample surface. The hardness varies, suggesting that the thickness of each layer in a multilayer system is important. The amount of ablated material during pulse generation plays an important role in achieving a high crystalline quality film.129
ZrC coatings were deposited on a SiC-coated graphite substrate using atmospheric (APS) and vacuum plasma spray (VPS) techniques.29 The formation of ZrO and Zr2O phases was observed due to the oxidation of ZrC powder in the APS process, giving rise to cracks and pores. On the other hand, the ZrC coating produced through VPS was devoid of oxides and exhibited a denser microstructure, smaller thermal expansion coefficients and higher thermal diffusivity, as compared with the APS-ZrC coating.
Zr-nitride coatings produced using the plasma-enhanced atomic layer deposition (PEALD) technique exhibited the formation of ZrO2 and/or oxynitride ZrOxNy due to ambient surface oxidation.81 Muneshwar and Cadien that such sputtering artifacts could lead to erroneous conclusions during nanoscale characterization.
Ion beam assisted deposition (IBAD) films show superior performance to other PVD techniques when low process temperatures are required to produce corrosion and wear resistant coatings for materials such as special heat-treated steels and aluminum alloys.138–143 Films produced using IBAD films possess high structural density and good adhesion. The bulk of the substrate is kept at low temperature during the bombardment of high energy ions.
Plasma sprayed ZrN coatings were produced in a controlled atmosphere.59 A nitrogen pressure of 700 Torr led to dense deposits with good interlamellar cohesion. The microhardness of the coatings varied between 945 and 1045 HV. At temperatures above 500 °C, oxidation modified the structures of the coatings, rendering them unsuitable for use.
Ion and electron beams from a plasma focus device were used to produce nanocrystalline zirconium carbonitride (ZrCN) coatings on zirconium substrates for multiple (10, 20, 30, 40 and 50) focus shots.144 Various phases including ZrN, Zr2N, Zr3N4, ZrC and Zr2CN were detected. The average crystallite size varied from 10 to 20 nm. A microhardness value of 5.6 GPa was observed for ZrCN composite films. The morphology of the coatings was affected by the number of focus shots. An improvement in the crystallinity of the Zr-nitride/carbonitride coatings was observed, which was attributed to the saturation of the residual stresses developed in all planes for higher numbers of focus shots (40–50), in turn caused by enhanced ion induced annealing of the substrate surface.
In another study using a DC magnetron sputtering technique,79 upon increasing the nitrogen flow rate from zero to 6.0 sccm (the argon rate was fixed at 6 sccm), the phase constitution of the coatings changed from α-Zr, α-ZrN0.28, ZrN, and Zr3N4 and finally to an amorphous phase. In another investigation using DC magnetron deposition, single-phase fcc-ZrN was observed at a nitrogen flow rate of up to 1 sccm. From 1 to 6 sccm, ZrN and Zr3N4 phases were detected, while an amorphous phase was identified above 6 sccm due to contamination with oxygen.80
Various zirconium nitrides including the metastable phases were deposited by varying the reactive gas composition and energy using dual ion beam sputtering.145 Use of low energy and a gas (Ar + N2) mixture resulted in the formation of Zr-nitride with metallic properties. High energy and pure nitrogen gas yielded a ZrN1.85 transparent insulator (physical properties similar to Zr3N4).
Low reactive gas flow rates (high Zr, low nitrogen) result in silver-colored metallic coatings.146 An increase in nitrogen to form stoichiometric ZrN imparts a golden color to the coatings.82,146 Nitrogen rich ZrNx coatings exhibit dark yellow, brownish yellow, dark brown and finally semi-transparent at N/Zr ratios of 1.2 to 1.3.146 In another study using DC magnetron sputtering deposition,79 the color of the coatings changed from silver to dark brown, then to green-yellow and finally to blue with increasing nitrogen flow rate. The golden color was not observed under the experimental conditions used in this study. Stoichiometric ZrN is a thermodynamically stable phase and known to possess a golden color, while Zr3N4 is metastable and mostly transparent.147 Deposition time affects the coating thickness but has a lower effect on the coating color.
In another study, the DC magnetron sputtering technique was used to study the composition, thickness and hardness of ZrN coatings deposited at different nitrogen partial pressures.67 Stoichiometric ZrN was formed at a nitrogen partial pressure of 28%. The thickness of the coatings deposited at a constant power decreased with an increase in nitrogen partial pressure. This occurs due to the surface poisoning of the target at higher nitrogen partial pressures, which serves to reduce the sputtering rate. All coatings were golden yellow in color. An increase in nitrogen partial pressure changed the shade from light to dark. Lower N2 partial pressures (7% and 11%) produced a (111) preferred orientation, while high pressures (14% and 28%) gave rise to ZrN with a (200) orientation.
ZrNx coatings with 200 nm thickness were deposited using RF magnetron sputtering with various nitrogen flow rates.148 The deposition flow rate decreased significantly from 0.34 to 0.1 nm s−1 between nitrogen flow rates of zero and 0.75 sccm. Any further decrease at high flow rates up to 10 sccm was negligible as seen in Fig. 5. The deposition rate decreased once a nitride layer formed at the surface of the Zr target. The sputtering yield of Zr was substantially higher than that of ZrN. The deposition rate was kept continuously low at higher nitrogen flow rates due to an increase in the system pressure, which served to lower the rate of diffusional mass transfer.148 The argon flow rate was fixed at 2 sccm, while the nitrogen rate was changed from 0 to 10 sccm during which ZrN films of silver, gold, brown, gray and green colors were produced. At high flow rates beyond the golden color, the aesthetics of the films was reduced and became unappealing for the decorative industry. Within a narrow regime of nitrogen flow from 0 to 0.75 sccm, the color of the film changed from silver, gold to golden brown. At a nitrogen flow rate of 3.5 sccm, the film exhibited a dark gray color. At ≥4 sccm nitrogen, the color was green.148 Dual ion beam sputtered Zr3N4 was reported to exhibit a blue color.149 The argon flow rate has an inconsequential effect on the color of the film.150
Fig. 5 Deposition rate of ZrN coatings decreases with increasing nitrogen flow rate during the RF sputtering process.148 (Reproduced with permission from ref. 148.) |
As the nitrogen flow rate is increased to 0.5 sccm, gold stoichiometric films of ZrN form with dominant (200) and (111) peaks along with weak (220) and (311) peaks. As the flow rate increases to 0.75 sccm, the (200) peak becomes stronger still. The surface roughnesses of both films are similar. At 1–3.5 sccm, the intensity of the (200) peak decreases significantly and the (311) peak disappears, while the film becomes grey. With increasing flow rate, the intensities of the (200) and (220) peaks decrease continuously.148 Simultaneously, the peaks keep shifting to smaller angles and become broadened, indicating the presence of polycrystalline ZrN and the progressive formation of Zr3N4.151,152 As the nitrogen flow increases to 4 sccm, the (200) peak disappears and a broad peak of Zr3N4 (320) is formed due to the incorporation of interstitial nitrogen. A continuous increase of nitrogen content forms a Zr3N4 phase and makes the structure of the film amorphous.
When the N/Zr atomic ratio is increased from zero to 0.5, the electrical resistivity increases.146 At these concentrations, nitrogen exists at interstitial sites of the Zr hcp lattice, which introduces grain boundaries and lattice distortion, thus increasing the electrical resistivity. At N/Zr ratios >0.5, phase transformation to ZrN starts to take place, which serves to decrease the resistivity to the values reported for the cubic ZrN phase. At N/Zr > 1, the electrical resistivity decreases rapidly.
Hollow cathode discharge ion-plating (HCD-IP) was used to deposit nanocrystalline ZrN films on Si(100) and AISI 304 stainless steel substrates.153 The deposition rate (and the film thickness) was higher for the SS substrate due to its high electrical conductivity. The thicknesses (350 to 550 nm) of the films with a columnar morphology changed with the deposition rate and were not related to the nitrogen flow rate that was varied from 5 to 35 sccm. The N/Zr ratio increased from 0.6 to 0.9 with increasing nitrogen flow rate since a larger number of nitrogen atoms are available in the chamber to react with Zr ions. The roughnesses of the films deposited on the stainless steel substrate were higher compared to those formed on the Si substrate. This was attributed to the higher surface damage caused by ion bombardment to the SS substrate compared to the Si surface at 450 C. Also, the larger substrate current density of the SS surface attracts more ions, resulting in more damage which presents itself as roughness in films.
All samples depicted a (111) preferred orientation.153 At higher nitrogen flow rates, (200) and (220) peaks appeared. The peak (220) became visible only at a nitrogen flow rate of >25 sccm. The (111) texture coefficient of ZrN decreased slightly for both substrates upon increasing the flow rate. The grain sizes of the ZrN films, measured at 15 to 30 nm, increased with increasing nitrogen flow rate. This could be due to the variation in pressure during deposition as the grain size of the film could be controlled by the mobility of adatoms during growth, which is influenced by the substrate temperature and ion impingement. Coatings yielded fine grain size despite the relatively high substrate temperature (450 °C) used in this study. Ion impingement, on the other hand, increases nucleation sites and decreases grain growth to result in fine grains.
The packing factor of ZrN/Si was observed to increase followed by a decrease, while the packing factor of ZrN/SS 304 first increased and then levelled off,153 as a result of a change in the flow rate of nitrogen. SS 304 is able to attract a larger number of Zr ions compared to Si. The larger number of Zr ions deliver higher energy and transfer momentum, which increases the mobility of adatoms to form a compact film. A smaller number of Zr ions are attracted by the Si substrate. The increase of the flow rate decreases the energy of the incoming Zr ions such that the adatoms no longer possess sufficient energy to form a dense film.
The hardnesses of the nanocrystalline ZrN films ranged from 23.3 to 26.6 GPa for coatings deposited on both substrates.153 The residual stress decreased and then increased with nitrogen flow rate. The hardness change was not related to the variation in the nitrogen flow rate or residual stress. Due to the fine grain size, dislocation pile-up or Hall–Petch hardening was not expected. The deformation mechanism of the ZrN films was thought to be grain rotation or grain boundary sliding and not slip by dislocations. In summary, Huang et al. concluded that the nitrogen flow rate changed the N/Zr ratio, packing factor and grain size of the films but had no significant effect on the film thickness, preferred orientation and hardness.
The ZrN films were deposited on polished flat M2 steel substrates by changing the nitrogen pressure and substrate bias voltage using an arc vapor ion deposition process.154 Dense columnar coatings with their main axis perpendicular to the interface were produced. The coatings became featureless under low pressure and low voltage deposition conditions. The (111) orientation dominated in the ZrN films at low concentrations of nitrogen. At 10 V and 33 μbar, a (200) preferred orientation was produced for coatings that exhibited high nitrogen content. The nitrogen concentration values were not reported in the paper. The changes in the orientation reflected the composition variation.
ZrN films with various stoichiometries were produced using the ion beam assisted deposition method.95 Stoichiometric ZrN was grown by using N/Zr ratios of 0.98–1.05. The preferred orientation of (111) along with (200) peaks were observed for these films. At N/Zr ratios of 1.1 to 1.26, a (220) preferred orientation was observed. The preferred orientation is influenced by ion bombardment in the high energy range. (220) planes grown parallel to the substrate are known to have low sputtering yields.155 Under high energy ion bombardment, (220) growth is preferred over the other planes since its re-sputtering rate is comparatively lower. Therefore, the (220) orientation was observed at relatively high N/Zr ratios of 1.1 to 1.26 due to the channeling effect. At a N/Zr ratio of 1.35, crystalline phases disappeared. Nitrogen atoms occupy octahedral sites in a stoichiometric ZrN phase. In over-stoichiometric ZrN, excess nitrogen atoms located randomly in tetrahedral sites result in dilation and amorphization.156,157
Thin zirconium nitride films were deposited on Si(100) substrates using ion beam assisted deposition.74 Arrival rate ratios (ARRs) (N/Zr) of 0.19, 0.39, 0.92, and 1.86 were used. The presence of metal Zr, nitride ZrN, oxide ZrO2, oxynitride Zr2N2O, and carbide ZrC phases was detected in the films. The relative amounts of these compounds were controlled by the ARR (N/Zr). The N/Zr ratio in the film increased with increasing ARR (N/Zr) until the latter reached 0.92. The excess nitrogen was rejected from the film. Contaminant oxygen and carbon were detected due to the better effect of zirconium.
The mechanical properties of coatings depend on their chemical and phase constitution and structure. Coatings with low nitrogen concentrations show reduced mechanical properties, while well-formed nitrides show superior mechanical properties. Moreover, the presence of an amorphous phase tends to deteriorate the mechanical behavior of the coatings. Dubey et al.116 evaluated the effect of the amount of nitrogen on the mechanical properties, rate of deposition and structural characteristics of zirconium tungsten nitride (ZrxW1−xNy) coatings, which strongly depended on pN2. Film deposition was carried out using a reactive magnetron sputtering technique. Structural, morphological, and cross-sectional analysis and characterization were undertaken using field emission scanning electron microscopy, transmission electron microscopy, shown in Fig. 6, atomic force microscopy, shown in Fig. 7, and grazing angle X-ray diffraction. Elemental composition analysis was carried out using energy dispersion X-ray analysis. It was recorded that for 0.33 Pa ≤ pN2 ≤ 0.67 Pa, ZrxW1−xNy films showed reflections corresponding to the (fcc + hcp) phase, for 0.20 Pa ≤ pN2 ≤ 0.27 Pa, an amorphous phase was obtained, and for 0.07 Pa ≤ pN2 ≤ 0.17 Pa, a single (fcc) phase was obtained. Non-monotonic variations of root mean square roughness and reduced film thickness were recorded with increase in pN2. The dual phase (fcc + hcp) film showed a maximum reduced modulus of elasticity (135 GPa) and hardness (∼24 GPa), while the single phase (fcc) film showed maximum ductility, wear resistance (H/Er2 ∼ 0.2 GPa) and fatigue fracture (H3/Er2 ∼ 0.87 GPa). High film adhesion to surfaces was exhibited by all film samples and no crack was propagated at a relatively high load of 50 mN.
Fig. 6 Selected area diffraction patterns and bright field image topologies of (a) a single fcc phase (0.13 Pa), (b) an amorphous phase (0.27 Pa) and (c) a dual (fcc + hcp) phase (0.47 Pa). (Reprinted from ref. 116 with permission from Elsevier.) |
Fig. 7 Atomic force microscope 3D × 2D topological images: (a) and (c) single phase (0.13 Pa) and (b) and (d) dual phase (0.47 Pa). (Reprinted from ref. 116 with permission from Elsevier.) |
Silva et al.117 researched the influence of nitrogen composition on the structural performances of ZrCN coatings with varying compositions of zirconium, nitrogen, carbon and oxygen in order to harness their potential for tribological applications. Nitrogen deposition from 2 to 10 sccm was used with DC reactive magnetron sputtering. The deposition rate of the ZrCN coatings decreased from 2.1 to 1.1 μm h−1 with increasing N2 flow due to the progressive poisoning of the targets. At a target potential of −400 V, a deposition rate of 0.7 μm h−1 was observed for ZrxN1−x. For the ZrxC1−x coatings, an inverse behavior was observed with a higher deposition rate of 1.8 μm h−1 and a lower potential of −280 V. The metallic coatings with Zr/(C + N) atomic ratios ≥2.9 exhibited a columnar morphology (see Fig. 8a) that is typical for porous coatings grown under low energy ion bombardment, limited adatom mobility and high deposition rates. They exhibited low hardness (13–15 GPa) due to their high Zr content. High coefficients of friction resulted in early failures in tribological tests. For Zr/(C + N) = 1.3, fcc ZrN coatings exhibited a (111) preferred orientation, and a fine-grained dense morphology (see Fig. 8b). The exhibited morphology is due to the decrease in the deposition rate brought about by target poisoning and increasing nitrogen content, which results in a transition from columnar metallic to fine-grained carbonitrides. The XRD peaks broadened and shifted to lower angles due to the C replacement of nitrogen atoms. A ZrCN solid solution phase was formed with hardness values close to 30 GPa. A compact structure resulted for the highest Young's modulus value. For Zr/(C + N) ≤ 0.7, coatings with a fine-globular morphology (see Fig. 8c) were produced due to the excess carbon and nitrogen that resulted in continuous re-nucleation of grains. The fcc ZrN-type structure was maintained but the (200) orientation became stronger with decreased crystallinity. The hardness was low (9–20 GPa) due to the formation of soft amorphous phases such as a-CNx and a-C. These phases resulted in low friction.
Fig. 8 Various morphologies of Zr-carbonitride films formed at Zr/(C + N) ratios of (a) ≥2.9, (b) 1.3 and (c) ≤0.7. |
As per the phase diagram,158 Zr–C–N can incorporate high amounts of N to form an α-Zr phase, while the C intake is small. Beyond 4 sccm flow of nitrogen, a face centered cubic ZrCN phase which served as a lubricant was formed. The best performance was found in coatings produced with 6 sccm flow of nitrogen with a wear rate of 2.27 ± 0.25 m3 N−1 Lap−1 × 1015.
A higher concentration of carbon (due to the increased methane content in the sputtering gas used during the reactive magnetron sputtering process) results in an increased hardness of coatings accompanied by a decrease in adhesion.23 Higher methane content increased carbon from 1000 to well over 3000 HV. A higher methane content was noted to increase the lattice parameters of the coating, as measured with XRD. This was attributed to the possible incorporation of carbon at interstitial sites in the ZrC lattice.23 The shift in the XRD peak could also be due to the change in the stress state of the coating due to its increased hardness. He et al.159 reported a maximum hardness of 31.5 GPa at a Zr/C ratio of 0.97. A further increase in carbon content reduced the hardness.
During the synthesis of Zr based coatings using cathodic arc deposition,160 it was indicated that the total gas flow rate as well as the CH4/(CH4 + N2) flow rate strongly affected the behavior and properties of the coatings. CH4/(CH4 + N2) ratios of 0.2 to 0.4 gave the highest hardness value (42–45 GPa) as compared to ZrC (19.6 GPa) and ZrN (29.1 GPa).
Varacalle et al.24 used air plasma spray to produce ZrC coatings. They concluded that a high secondary flow of hydrogen and current during processing resulted in coatings with the highest hardness and thickness, and with the lowest porosity. Various textures of ZrC coatings such as (002), (111)129 and (111), (220)23 have been reported. The change in substrate temperature and gas pressure is thought to influence the preferred orientation of the coatings.23
Meng et al.40 reported the structure of ZrC films to consist of nanocrystalline ZrCx grains embedded in a matrix of amorphous carbon (a-C). For carbon contents above 86 at%, a crystalline ZrCx phase was not observed. A large amount of a-C resulted in a reduced hardness and an increased resistivity of the film. Concurrently, improvements in the friction coefficient and wear resistance were also observed. Fig. 9 shows the coefficients of friction curves for coatings with various carbon concentrations against Si3N4. It can be seen that the friction coefficient decreased upon increasing the carbon content from 44 to 88 at%, which was attributed to the presence of an amorphous carbon phase.
Fig. 9 Friction coefficient curves for coatings with 44–88 at% carbon concentrations against Si3N4 balls as a function of sliding cycle. (Reproduced with permission from ref. 40.) |
Examination with SEM revealed the wear tracks obtained from the coatings against Si3N4 balls after 10000 laps as shown in Fig. 10. It can be seen that the wear track for the sample with lower carbon content is broader compared to the other, suggesting a loss of the material due to wear.
Fig. 10 SEM images of the wear tracks and profiles obtained from coatings with (a) 44, (b) 60, (c) 82, (d) 86 and (e) 88 at% carbon against Si3N4 balls after 10000 laps. (Reproduced with permission from ref. 40.) |
Resistance to plastic deformation is defined by the H3/E2 ratio. High values of this ratio denote high wear resistance. It can be seen in Fig. 11 that the H3/E2 ratio increases with carbon content.
Fig. 11 H3/E2 as a function of carbon concentration in the coatings. (Reproduced with permission from ref. 40.) |
A larger sp2/sp3 ratio of the a-C phase relieved stress and improved the electrical properties. The Zr-based films exhibited lower friction coefficients than nanocomposite films based on Ti.
Larijani et al.121 researched the effect of the methane (CH4) flow ratio on the micro-nano-structure and hardness of carbonitride coatings deposited on AISI 304 stainless steel by an ion beam sputtering method. Rutherford backscattering, scanning electron microscopy and X-ray diffraction were used to investigate the coatings. The substrate temperature was 400 °C and the working pressure was maintained at 8 × 10−5 Torr. It was shown that an increase in the methane flow ratio changed the crystallographic texture and phase composition of the coating. The crystallographic texture changed from (111) to (220) and the ZrN crystalline phase shifted towards a ZrC crystalline phase via an intermediate phase of ZrN1−xCx, where 0 ≤ x ≤ 1. The maximum hardness was 2520 Hv for x = 0.57 based on the Vickers hardness test. Bruckner et al.23 noted that increasing the methane partial pressure changed the structure of the ZrC coating from ‘fibrous’ to ‘open’, while the surface was transformed from smooth to flaky. Moreover, increasing the methane content decreased the deposition rate.
Grigore et al.104 presented ZrCN coatings deposited by a duplex process that combines ion implantation and magnetron sputtering with a view to analyzing the effect of hydrocarbon (butane) and nitrogen reactive flow rates on the morphologies, chemical compositions and structures of coatings under different deposition conditions. For this purpose, glow discharge optical emission spectrometry (GDOES), X-ray diffraction and scanning electron microscopy (SEM) techniques were employed. The range of the microhardnesses of the coatings obtained was 3180 to 4050 HV0.05. A C/N atomic ratio of 0.9 exhibited the highest microhardness but the least wear resistance values, while the coatings that exhibited the least hardness showed better wear resistance properties.
Craciun et al.129 researched the mechanical properties of zirconium-based coatings grown by pulsed laser deposition (PLD). ZrC/TiN, ZrC/ZrN and ZrC coatings were grown on Si(100) substrates at a temperature of 573 K by PLD. The cooling rate was 278 K min−1. Auger photoelectron spectroscopy (AES), as shown in Fig. 12, X-ray photoelectron spectroscopy (XPS), X-ray diffraction (XRD), as shown in Fig. 13, and X-ray reflectivity curves were employed for analysis. The results showed that the gas pressure and the nature of the gas used during deposition determined the grain sizes of the deposited crystalline films. The surface morphology and density of the coatings showed marginal improvement when the central part of the laser was used for deposition using an aperture.
Fig. 12 AES spectrum acquired from the bulk region (after 5 min sputtering) of the ZrC/ZrN multilayer sample. (Reprinted with permission from ref. 129.) |
Fig. 13 Symmetrical XRD (upper traces) and GIXD (lower traces) patterns collected from three different locations on the ZrC/ZrN multilayer sample. (Reprinted with permission from ref. 129.) |
ZrC, TiN, and ZrC/TiN multilayer crystalline coatings with a maximum thickness of 400 nm were grown on Si(100) substrates at 300 °C using a pulsed laser deposition (PLD) technique with a KrF excimer laser.46 The nanoindentation hardness of the multilayers was between 35 and 38 GPa, higher than the 30–33 GPa for single layers of ZrC and TiN. The grain size of the Zr coatings was measured between 8 and 10 nm using XRD and TEM. In theory, an inverse Hall–Petch effect is activated for ZrC at or less than 9.4 nm grain size, where the hardness shows a decreasing trend.161,162 However, such an effect was not observed in this study.
The properties of ZrC/ZrN and ZrC/TiN multilayer structures prepared using pulsed laser deposition were investigated.47 The use of an Ar atmosphere during deposition resulted in predominantly equiaxed grains in the ZrC/TiN coating with less texture. Under a CH4 atmosphere, a low pressure of 2 × 10−3 Pa produced the best results. It also appeared that the larger thickness of the bilayer produced higher hardness values.
DC unbalanced magnetron sputtering was used to produce ZrCN films with a total flow rate of C2H2 and N2 of 15 sccm.163 The hardness and wear behavior of δ-Zr(CxN1−x)1−y films depended on the variation in the C2H2/N2 ratio.
The film showed a (111) preferred orientation. The film phase, structure and orientation remain unaffected by variations in the C2H2/N2 ratio within the deposition conditions used. The addition of Ti and W caused broadening of ZrCN XRD peaks with no peak shift. New peaks belonging to αW2C, W and TiCN were identified. Additions improved the hardness and wear performance due to the formation of new phases in the film. Ti addition produced better results than W addition. ZrCN, with and without Ti/W additions, showed much better wear performance than TiN.
A combined magnetron sputtering and ion implantation process with nitrogen and hydrocarbon (butane C4H10) reactive gases was used to deposit zirconium carbonitride coatings.104 In this technique, in addition to the DC bias voltage, negative high voltage pulses of 25 Hz were applied periodically to the substrate. High hydrocarbon flow rates resulted in the formation of Zr2CN, Zr2N, ZrC0.6 and ZrC. The diffraction lines shifted to lower angles due to the large number of carbon and nitrogen atoms at interstitial positions. The coating grains were columnar with 10–16 μm thickness. Coatings with microhardnesses in the range 3180–4050 HV0.05 were obtained depending on the deposition conditions. These values are higher than those reported for similar coatings produced with magnetron sputtering163 or those cited for hot pressed carbonitride powders.164 The wear tests indicated that the coatings with a C/N ratio of 0.9 exhibited the highest microhardness (4050 HV0.05) and their wear resistance was the poorest, while the coatings with a lower microhardness exhibited better wear resistance.
Oxygen content in the coatings is influenced by the substrate bias. For DC sputtered ZrN films, the deposition rate decreases monotonically from a positive to negative substrate bias because the deposited species are re-sputtered by energetic argon ions.146 The nitrogen and oxygen concentrations in the coatings decrease as the positive bias increases. This could be attributed to two reasons. Firstly, at constant power, application of positive bias to the substrate increases the negative bias applied to the target. As a result, a larger number of positive argon ions bombard the target, which leads to increased sputtered Zr atoms in the plasmon. The ionized Zr ions also lose momentum while moving toward the substrate due to an opposing electric field. Secondly, the positive substrate bias attracts more electrons relative to ions toward the substrate, which serves to neutralize nitrogen ions, thus inhibiting the nitride interactions. The electrical resistivity decreases initially and then increases progressively with positive bias as shown in Fig. 14. This is related to the composition change where the N/Zr ratio decreases to 0.5 for a bias of +50 V, where metastable Zr2N is observed. An increase in positive bias results in a rapid decrease in the (002) texture due to the higher deposition rate. The oxygen decreases and the nitrogen remains nearly unchanged upon increasing the negative bias. The electrical resistivity decreases linearly with negative bias, which is due to the increase in crystallinity and the decrease in oxygen concentration. The increase in negative bias results in a gentle decrease in the (002) texture.
Fig. 14 Influence of the substrate bias (DC power = 150 W) on the resistivity and composition of ZrNx films. (Reproduced with permission from ref. 146.) |
Zirconium nitride films were deposited on silicon(100) substrates using direct current reactive magnetron sputtering.75 At a DC negative bias voltage of −26.3 V, a significant (200) preferred orientation in the film was observed. The ZrN diffraction peaks were shifted toward a high angle compared to bulk ZrN, indicating the presence of tensile stress in the film. At a substrate voltage of −80 V, the preferred orientation was (111). The diffraction peaks shifted toward a low angle, indicative of compressive stresses. At −160 V, the (111) preferred orientation became more dominant. At −400 V, the formation of an over-stoichiometric Zr3N4 phase was observed. Thermodynamic calculations revealed that high surface energy promotes the (200) orientation, while high strain energy favors the (111) orientation. At a low substrate voltage, the difference in surface energy between (200) and (111) is high (1.85 MPa), while the difference in strain energy is low (0.002 MPa); thus the (200) orientation is preferred. As the voltage is increased from −80 V to −320 V, the difference in the strain energy increases, while the surface energy remains constant, giving rise to a (111) preferred orientation. At −400 V, the strain energy becomes adequately high to drive a phase transition from ZrN to Zr3N4. The driving force for the phase transition is considered to be the decrease in strain energy since Zr3N4 has lower strain energy than ZrN.
Nanocrystalline ZrN films were deposited on Si(100) and AISI 304 stainless steel substrates using hollow cathode discharge ion-plating (HCD-IP).167 The ZrN films were close to the stoichiometric composition. The ZrN films deposited on the stainless steel were very smooth, with their roughnesses ranging from 1.1 to 3.9 nm. The columnar structure of the ZrN film became denser with increasing bias. Continuous bombardment of energetic ions serves to peen and compact the film to near bulk density. The presence of a columnar morphology indicates that the energy of ions is not adequate to produce near-bulk compact structures. The width of the columns was 50–100 nm and the length was 250 nm. A cauliflower-like structure was also observed and it was attributed to the low mobility of adatoms and the shadowing effect. Coating thickness was not related to substrate bias.
Zr-nitride films exhibited a (111) preferred orientation on both Si and SS 304 substrates. Zr-nitride films have a strong tendency for a (111) orientation as it is dependent on the atomic mass of the metal in the NaCl-type metal nitride.168 The ion bombardment of heavy ions such as Zr ions favors (111) growth. It was observed that the FWHM measured in XRD experiments decreased (i.e., the crystalline quality of the ZrN films improved) with increasing bias. The increased negative substrate bias results in increased ion bombardment, giving rise to momentum transfer or energy deposition in a certain volume on the surface. This in turn facilitates the movement of adatoms at the surface to equilibrium lattice sites and thus enhance the crystallinity of the film.169 The hardness values of ZrN films deposited on Si ranged from 27 to 30 GPa, and those on 304 stainless steel were from 32.5 to 40.8 GPa.168 The substrate bias was not found to have a significant effect on hardness values. The high hardnesses of the films on SS 304 were attributed to the high residual stress in the film, which is due to the large thermal expansion coefficient between the film and the SS substrate. The resistivity is related to the lattice defects in the ZrN film. The resistivity of the ZrN films gradually decreased upon increasing the bias up to −120 V, after which it increased abruptly. The increase in ion bombardment due to the increased bias results in the movement of adatoms to equilibrium sites, increased film compactness and decreased lattice defects. All these factors serve to decrease the resistivity and increase the crystallinity of the film. On the other hand, over-stoichiometric films can show increased resistivity due to the larger density of defects. High energy ions could induce lattice defects too. The abrupt increase observed in the resistivity at high bias voltages could be for the above-stated reasons. The corrosion resistance of ZrN-coated stainless steel in 5% NaCl and 1 N H2SO4 + 0.05 M KSCN solutions increased with the bias ranging from 0 to −90 V, then abruptly decreased at −120 V, and then increased again at −150 V. Similar to resistivity, the corrosion behavior was explained by the change in film structure due to bias-induced ion bombardment.167
Stoichiometric columnar ZrN films were deposited on Si(100) substrates using the hollow cathode ion-plated (HCD-IP) technique.170 The thickness of the film was also controlled. The substrate bias was varied from floating to −300 V. The crystallinity improved with increasing negative bias. The ZrN films showed a (111) orientation from 0 to −250 V. At a bias voltage of −300 V, the (220) orientation became the preferred orientation. The change in the orientation was related to the energy delivered to the film. At high ion energy, ion damage or ion channeling of (111) is higher than that of (220) under perpendicular ion bombardment. This results in a change in the preferred orientation from (111) to (220). The hardness values of the ZrN films ranged from 22 to 32 GPa. The films with the (111) preferred orientation are expected to show higher hardness. The active slip systems in ZrN (NaCl-type structure) are of the {110} 〈110〉 family.171 If the applied force is perpendicular to the (111) plane, the resolved shear stress on all slip systems becomes zero. In this way, the primary slip systems are not activated and thus higher hardness is attained. For films with the (220) preferred orientation, the external force is perpendicular to the (220) plane, and only half of the slip systems have a zero Schmid factor, giving rise to lower hardness values. The packing factor increases with increasing negative substrate bias and reaches a maximum value at bias −50 V, then decreases with increasing negative bias.170 The increasing bias increases the ion bombardment which results in higher packing density. At increasingly higher bias, the high energy ions introduce defects into the growing film, thereby decreasing the packing density. Similarly, resistivity is also related to lattice defects and follows the same trend as the packing factor. Moreover, a linear relationship was observed between brilliance and the packing factor. At a substrate voltage of −50 V, the ZrN films showed the lowest resistivity of 56 mV cm, the highest packing factor of 0.99, the lowest roughness of 0.66 nm, the highest brilliance of 87.2, and a relatively high hardness of 30.63 GPa.
The dual cathodic arc ion deposition technique was used to grow ZrN on glass and aluminum substrates.172 The ZrN film prepared at a bias voltage of −100 V was 282 nm in thickness. At −400 V, the measured thickness was 259 nm. The film thickness decreased due to the increased re-sputtering of the deposited film material with increasing negative bias.173 With a change from −100 V to −400 V, the films became more stoichiometric values (the N/Zr ratio changed from 0.851 to 0.923). At a constant bias of −400 V, as the argon concentration was increased (to N2/(Ar + N2) = 15%), the N/Zr ratio decreased significantly to a low value of 0.215. Concurrently, the ZrN film thickness increased from 259 to 351 nm. The marked increase in the growth rate was attributed to the increased yield rate at the target. It was stated that a smaller growth rate at high nitrogen concentrations was due to the lower evaporation rate at the target with nitride formation.
ZrN coatings (3.5 μm in thickness) were deposited on steel and silicon substrates using magnetron sputtering.71 Application of a bias voltage produced films with a (111) preferred orientation, while (200) growth was observed once the bias was removed. For 0 to −110 V, the lattice constant increased due to nitrogen over-stoichiometry. For negative bias voltages higher than −110 V, the lattice constant decreased due to the preferential re-sputtering of nitrogen. Also, porosities and an increase in film surface roughness were observed due to the re-sputtering phenomenon. The average crystal size was 7 to 9 nm. Unbiased films had 21.8 GPa hardness, which remained unaffected with the variation of the nitrogen and argon flow rates of 3, 4 or 5 sccm and 5, 15 and 25 sccm, respectively. However, at −80 to 90 V, the hardness increased to 27 GPa. The maximum hardness of 39.5 GPa was observed at a bias of −100 V. The hardness decreased to 33 GPa with a further increase in bias. It was stated that at low negative bias the film density increased due to the elimination of voids, which increased the hardness. A further increase in bias induced re-sputtering that reduced the hardness. Compressive stresses were also observed to increase with negative bias.
Application of substrate bias in the reactive magnetron sputtering process increases the target voltage, probably leading to a higher Zr content and a lower nitrogen content in the coatings. It does not, however, cause any variation in deposition pressure, deposition rate and growth mode.82
Zr–ZrC–ZrC/DLC gradient composite films were deposited on TiNi alloy using combined plasma immersion ion implantation and deposition (PIIID) and plasma enhanced chemical vapor deposition (PECVD).28 XPS results indicated that the composition of ZrC depended heavily on the bias voltage. With the increase of bias voltage, the content of ZrC and the sp3/sp2 ratio first increased, reaching a maximum value at 200 V, and then decreased. Similarly, the hardness and elastic modulus of the coatings reached a maximum value of 13 GPa and 200 GPa, respectively, at 200 V, and then decreased gradually until reaching a stable value of 9 GPa and 100 GPa, respectively. The microscratch curve tests showed critical loads of 60 N, which showed that the coatings had excellent adhesion.
RF magnetron sputtering at different bias voltages was used to prepare ZrN films on tungsten carbide substrates.83 Scratch and ball-on-disk tests were employed to test the adhesion and wear resistance of the coatings. Adhesion to the WC substrate was improved in that the coatings showed higher critical load and scratch hardness along with a lower wear rate at an optimal bias voltage of −5 V when compared to coatings grown with no bias or with higher negative bias voltages (see Fig. 15). Wear tracks formed at the surfaces of samples are shown in Fig. 16. It was concluded that appropriate substrate voltage bias played an important role in the improvement of the tribological properties of the coatings.
Fig. 15 Plot depicting the wear rate versus bias voltage. (Reproduced with permission from ref. 83.) |
Fig. 16 SEM images of wear tracks formed on samples: (a) ZrN with 10 N load and (b) ZrN with 5 N load. Insets: High magnification images near the track edge. It can be seen that larger loads produced greater material removal. (Reproduced with permission from ref. 83.) |
ZrC thin films were grown on a silicon(100) substrate using the reactive magnetron sputtering process. The substrate temperature used was from ambient to 500 °C. At less than 300 °C, ZrC consisted of ZrC nanocrystallites embedded in amorphous carbon, while at higher growth temperatures the films were highly textured. The hardness and elastic modulus increased with temperature with a maximum of 24.8 GPa and 213 GPa, respectively, at 325 °C attributed to the decrease in grain size and the increase in sp3 bonding compared to sp2 bonding in ZrC as shown by an XPS study.42
Nanocrystalline ZrC coatings with grain sizes from 6 to 20 nm were grown on Si(100) substrates at temperatures from 30 to 500 °C by the pulsed laser deposition technique.45 The coatings were under compressive residual stress. Nanoindentation hardness values of above 40 GPa were recorded for ZrC coatings prepared at substrate temperatures higher than 300 °C. It was concluded that high hardness values are achieved for highly dense and nanocrystalline coatings.
In another study,34 ZrC particulates with 5 nm grain size were observed to grow in the (111) preferred orientation at a growth temperature, Ts, of 400 °C. The morphology became smooth as the temperature was increased. It was observed that the growth temperature did not affect the nanoindentation hardness and elastic modulus. Improved adhesion, corrosion resistance and hemocompatibility were recorded for coatings deposited at 200 °C and 400 °C compared with ambient temperature.
Zirconium carbonitride thin films were deposited on steel substrates by means of the dc plasma-assisted chemical vapor deposition technique using metal organic compounds as precursors.103 At 200 °C the desorption rate was too low to prevent the incorporation of organic fragments in the growing films. Therefore, the metal content of the films remained sub-stoichiometric. The concentrations of oxygen and organic bonded carbon impurities in the films decreased at deposition temperatures above 250 °C. At <300 °C, the films depicted a columnar morphology, a maximum growth rate and a Vickers hardness of 2000 HV. At a substrate temperature of 400 °C or below, dense homogeneous fine grained polycrystalline Zr(C,N) coatings were obtained. At >400 °C, powdery layers were produced due to the decomposition of the precursor in the gaseous phase owing to the low stability of the metal organic compound at elevated temperatures.
Radio-frequency magnetron sputtering was used to produce zirconium carbonitride coatings on AISI 316L austenitic stainless steel.110 Coatings were almost amorphous at a growth temperature of less than 400 °C, while nanostructured Zr2CN with a (111) preferred orientation was formed at Ts of 400 °C. This was accompanied by an increase in the nanohardness from 17 GPa to over 32 GPa, an increased elastic modulus and better adhesion. The mobility of adatoms improved at higher Ts and impinging particles with more energy contributed to the formation of a close-packed structure in a state of near thermodynamic equilibrium. Moreover, higher Ts contributed to the reduction in defects while (111) grain texture was formed, resulting in an increase in adhesion.
In another study, Mg- and Al-based alloys were successfully coated with ZrCN and TiCN layers at low substrate temperatures between 110 and 200 °C.137 The deposition temperature was kept low to avoid reaching the hardening temperatures of these alloys. High substrate temperatures and high bias voltages used along with high C concentrations during the reactive magnetron sputtering process resulted in dense, smooth and hard ZrC coatings.23 The increased bias voltage decreased the deposition rate, the film structure became denser, and the argon content in the film increased.23
The influence of temperature on the chemical and mechanical performances of multi-element (AlCrTaTiZr)N coatings prepared by RF reactive magnetron sputtering was studied by Chia-Han Lai et al.115 Nitrogen and argon flows were kept constant, while the substrate surface temperature ranged between 100 and 500 °C. X-ray diffraction (XRD) was employed for analysis. Single-phase face-centered-cubic structure was recorded, and the results of analysis showed that the elastic modulus (350 GPa) and hardness (35 GPa) of the researched material were relatively independent of substrate temperature. The elevation in substrate temperature resulted in a monotonic decrease in compressive internal stress from 3.2 to 2.0 GPa; decrease in nitrogen concentration, lattice parameter, and crystallite size; and increase in (200) peak intensity.
The tribological behavior of ZrN coatings deposited on titanium modified austenitic stainless steel (alloy D-9) using the pulsed magnetron sputtering technique at 27–600 °C was investigated.78 The ZrN coatings prepared at higher deposition temperature showed lower coefficients of friction.
The deposition rate increases with DC power used during the DC magnetron sputtering of ZrN films.146 The reaction rate of nitrogen with Zr decreases because the number of sputtered Zr atoms increases. The stoichiometry region for the formation of ZrN slightly broadens and moves toward a higher nitrogen flux ratio.
Ion assisted deposition was used to prepare ZrN coatings at various ion beam energies.174 The optimum growth conditions were an ion energy of 150–200 eV, a N/Zr ratio of 1.2–1.5 and a substrate temperature of 820 °C. ZrN coatings developed using the ion beam assisted deposition technique exhibited (111) and (200) preferred orientations at beam energies of 500 V and 700 V respectively.70
Chen et al.125 researched the influence of the chemical concentration ratio (Cr/Z ratio) on the Daimler-Benz Rockwell-C (HRC-DB) adhesion, nanoindentation, microhardness, roughness, wear resistance and scratch resistance of the multilayer CrN/ZrN coatings that were deposited using a cathodic arc system. The Cr/Zn atomic ratio was controlled in the range of 1 to 2.5 by using various values of target current. The phase and concentration of the CrN/ZrN multilayer were analyzed using a glancing angle X-ray diffractometer and a field emission electron probe micro-analyzer (FE-EPMA) respectively. It was shown that the Cr/Zr chemical composition ratio remarkably affected the tribological and hardness performances of CrN/ZrN multilayer coatings. The maximum coating hardness (about 28 GPa) was achieved with a Cr/Zr atomic ratio of 2.1. The occurrences of reflections of the (111), (200), (220) and (311) indices were recorded for ZrN single layer coatings. For CrN/ZrN multilayer coatings, even though some characteristic reflections were seen, different XRD reflection intensities were noticed. In addition to these observations, reflections along the ZrN(111) plane were produced in multilayered thin films.
Braic et al.118 investigated the effect of adding Nb, Hf and Ti to ZrCN based coatings. Base coats of two different metal ratios were used: highly stoichiometric ((Me1 + Me2) ∼ 3) and quasi-stoichiometric ((C + N)/(Me1 + Me2) ∼ 1) where films are composed of metals Me1 and Me2. Coating preparation was undertaken using the reactive magnetron sputtering technique with the aim of investigating their wear resistance, hardness, surface morphology, texture and phase compositions. Nanocomposite structures were observed in the films. The structures consisted of amorphous carbon and crystalline metal carbon nitrides. The quaternary coatings showed better wear resistance and mechanical properties. The lower the metal content, the lower the friction coefficient, the higher the hardness and the finer the morphology. Lower deposition rates were recorded with decrease in metal content. Coatings with equal metal and non-metal ratios exhibited similar Raman spectra. The spectra for metals containing carbon films, carbon nitride, and amorphous carbon were similar and they showed a graphite structure. Increases in the D & G peaks in the Raman analysis were noticed with increase in carbon content for both coating types and for all metals. The friction coefficient μ versus sliding distance of the deposited film is shown in Fig. 17 and it was discovered that the films with high concentrations of non-metal showed lower friction coefficients.
Fig. 17 Friction coefficients (μ) and sliding distances of ZrCN, (Zr,Ti)CN, (Zr,Hf)CN and (Zr,Nb)CN coatings: (a) low non-metal content and (b) high non-metal. (Reprinted from ref. 118 with permission from Elsevier.) |
Balaceanu et al.160 evaluated the corrosion resistance, tribological, adhesion, hardness and surface roughness properties, texture, chemical bonding, phase and elemental compositions of super-hard ZrCN based coatings deposited on high speed steel, plain carbon steel and Si substrates by a cathodic arc method. Al and Ti were added to the base coatings to check for their effects on the above properties. Coating characterization was carried out by X-ray diffraction (XRD), GDOES, and XPS techniques, amongst others. The addition of Al and Ti to ZrCN resulted in the improved properties of TiAlCN, ZrCN, ZrC and ZrN based coatings.
Long et al.130 examined the mechanical properties, microstructure and phase composition of Zr-carbide coatings (ZrC and ZrC0.85) deposited by means of chemical vapor deposition. For this purpose, X-ray diffraction (XRD) and X-ray photoelectron spectroscopy (XPS) were used for analysis. Hardnesses of 22–28 GPa and Young's moduli of ∼303–321 GPa were reported for stoichiometric (ZrC) coatings, which are more than those of non-stoichiometric coatings (ZrC0.85). Cubic ZrC was formed and a strong (200) texture normal to the surface of the substrate was exhibited in both coatings. Compared to the stoichiometric ZrC, the peak position corresponding to the (200) reflection in the non-stoichiometric coating (ZrC0.85) was closer to the 2Θ value and the lattice parameter was slightly lower. The presence of both Zr and C at the surface of the coating was confirmed with XPS. The binding energies for ZrC and ZrC0.85 related to the Zr 3d peak were different, thus confirming the change in stoichiometry within ZrC. Peaks corresponding to oxygen present due to contamination were also observed, confirming the existence of the Zr–O bond (Fig. 18).
Fig. 18 XPS results obtained from ZrC coatings showing (a) a survey spectrum with peaks representing various energy levels. (b) Variation of intensity at core-levels in stoichiometric ZrC and non-stoichiometric ZrC0.85 corresponding to Zr 3d. (Reproduced with permission from ref. 130.) |
At low deposition rates, coatings are columnar and large in thickness. At high rates, coatings become dense and featureless. The chemical constitution of the coatings is heavily influenced by the deposition flow rate of reactive gases such as nitrogen. For instance, as the rate is increased, the phase constitution changes from α-Zr, α-ZrN0.28, ZrN, Zr3N4 and finally to an amorphous phase.
The hardness of ZrCN coatings is affected by the carbon content and it increases with increase in carbon content and discharge voltage. It was reported that the hardness of ZrCN and Zr/ZrCN films was improved with increasing carbon concentration. A low nitrogen flow rate results in a metallic silver color, while increased nitrogen supply imparts a golden color to the coatings. At high nitrogen partial pressures, the film thickness decreases due to the surface poisoning of the target. The electrical resistivity changes with the flow rate depending on the phase constitution of the coating. The hardness of the coatings also depends on the grain size, structure, defects, preferred orientation, residual stresses and chemical and phase constitution of the coatings. A high Zr content in the coating leads to reduced hardness. The formation of soft amorphous carbon or CNx exhibits low hardness, friction and high resistivity. Over-stoichiometric films also exhibit higher resistivity. For ZrCN coatings, a C/N ratio of 0.9 gives high hardness. Generally, (111) and (200) preferred orientations are observed for stoichiometric ZrN and over-stoichiometric ZrN, respectively.
An increase in negative bias voltage at the substrate may influence the preferred orientation, phase constitution, hardness and degree of crystallinity. At a low negative voltage, the (200) orientation is preferred. At a high negative voltage, the (111) orientation is preferred. With increasing voltage, the crystallinity increases, the phase changes from ZrN to Zr3N4 and the columnar coating structure becomes denser, in turn increasing the hardness. The coating thickness is reduced due to the re-sputtering effect.
The grain size of the Zr-based coating increases with increasing substrate temperature unless repeated re-nucleation occurs. The hardness decreases and the fracture toughness increases as the temperature increases. Better adhesion occurs at temperatures greater than ambient temperature. An increase in substrate temperature results in a decrease in compressive stress, nitrogen concentration, lattice parameters, and crystallite size and an increase in (200) peak intensity in multi-element nitride coatings.
Increased ion energy results in a change in the preferred orientation from (111) to (220) for ZrN. It also favors build-up of compressive stresses. The longer the deposition distance, the smaller the deposition rate. The same duration will give different coating thicknesses due to the poisoning of the source.
Based on existing work, much research needs to be carried out on Zr-based coatings in the areas including cost-effective and easily controlled methods of preparation, energy consumption, condensation challenges in PLD techniques, etc. Likewise, induced porosity, oxidation introduced by the coating processes, altered substrate properties, use of multi-deposition methods, minimization of coating property trade-offs during optimization, and multilayered coatings make interesting topics of research.