Mengjie
Zhang
,
Wenchang
Zhu
,
Xingzhe
Yang
,
Hao
Chen
and
Hongbin
Feng
*
Institute of Materials for Energy and Environment, School of Materials Science and Engineering, Qingdao University, Qingdao 266071, China. E-mail: fenghongbin@qdu.edu.cn
First published on 31st August 2020
The uniform and surfactant-free synthesis of ultrafine alloy nanoparticles (NPs) still remains an ongoing challenge. Here, we developed a general route for synthesizing sub-3 nm nanoalloys on a carbon support via a shear-assisted liquid-metal reduction (SA-LMR) strategy. The utilization of shearing treatment resulted in the rapid release of electrons from the liquid sodium-potassium (NaK) alloy, which enabled the ultrafast reduction of precursor metal ions to metallic nanoalloys at room temperature. As a model system, Pt–Cu NPs with uniform distribution were synthesized and characterized by spectroscopic and microscopic techniques. The size, composition and structure of the Pt–Cu NPs could be tuned by controlling the volume of liquid NaK alloy and the reaction time. To prove the universality and utility of our method, the binary Pt–M (Fe, Co, Ni, and Cu) and ternary Pt–Cu–Fe nanoalloys deposited on a carbon support were prepared as hydrogen evolution reaction (HER) catalysts. This facile, rapid and universal synthesis technique has the potential to be employed in the large-scale production of nanomaterials and suggests a new direction for nanoalloys.
Commonly, the wet chemistry synthesis of well-dispersed alloy NPs needs the assistance of organic surfactants or capping agents, such as cetyltrimethylammonium chloride, ethylene glycol, oleic acid, or oleylamines, to protect them from agglomeration.28–33 Nevertheless, the residual surfactants are often difficult to remove completely, which makes it difficult to obtain nanocrystals with clean surfaces.34 Especially for catalytic applications, the active sites are occupied, which prevents the adsorption of reactants and leads to a decrease in the catalytic activity. So, a general and facile method that can easily control the nucleation and growth of uniform and ultrafine alloy NPs with clean surfaces is highly desirable.35–38 Recently, Sheng Hu et al. reported a method for the synthesis of intermetallic nanoparticles without using surfactants via laser ablation in a solution-galvanic replacement reaction and achieved good electrochemical performance.39–41 As in the general case for nanocrystal synthesis, the speed of the nucleation process is critical for controlling the uniformity of NPs. To obtain uniform and ultrasmall nanocrystals, nucleation must occur rapidly and instantaneously. Fast nucleation is easily achieved by the rapid reduction of metal ions using a strong reductant. However, the ultrafast, uniform, and surfactant-free synthesis of ultrafine nanoalloys in a strong reduction reaction system remains a challenge.
Here we report an ultrafast and surfactant-free approach for the preparation of alloy NPs with controllable size and composition by using a shear-assisted liquid metal reduction (SA-LMR) strategy at room temperature. A very active liquid metal, sodium–potassium (NaK) alloy, was first used as a rapid and effective heterogeneous reductant for the general synthesis of metallic nanoalloys via a redox substitution reaction. The entire reaction process does not require the addition of surfactants and so can avoid the particle agglomeration problem. When the highly active liquid NaK alloy reductant was used, a burst-nucleation was achieved at room temperature, in which the concentration of monomers in the solution rose rapidly to reach the concentration of nucleation, thereby shortening the nucleation time and ensuring that the size of the nanocrystals tended to be uniform. The kinetics became sufficiently fast, and the reaction time was very short (∼30 s), dramatically shorter than in previous reported studies using wet chemical synthesis.29,31 Additionally, with the simplicity of the shear-assisted process, the synthesis could be easily scaled up while maintaining the uniformity of the particle size, as well as homogenizing the reducing agent, precursor, and the carbon supports. This facile, universal, and large-scale potential technique provides a new route for the synthesis of uniform metallic alloy nanoparticles and can shed light on further innovation in nanocatalysts.
![]() | ||
Fig. 1 Scheme for the synthesis of ultrasmall Pt–Cu nanoparticles in the strong reduction non-aqueous system by a shear-assisted liquid NaK alloy reduction process. |
In order to reveal the nucleation and growth process of the alloy NPs in our system, taking Pt–Cu nanoalloys as an example, we synthesized a series of Pt–Cu alloy NPs on the carbon support (Pt–Cu-xvc72) with different sizes by regulating the reaction time (tR) and the amount of liquid NaK reducing agent (VR). The transmission electron micrograph (TEM) images (Fig. 2a–i and S1†) showed the morphologies and the size changes of a series of Pt–Cu alloy NPs on carbon black that were related to the VR and tR in the reaction system. When the tR and other conditions were kept constant, the more the VR added to the system, the larger the size of the Pt–Cu NPs formed by the reaction. Fig. 2a–e display the TEM images of Pt–Cu NPs and their particle-size variation along with the changes of VR from 10, 20, 40, and 80 μL to 160 μL, respectively, when the tR was constant at 10 s. As shown in the insert images in Fig. 2a–i, on the basis of the TEM observation, we measured the size of different 100 nanoparticles (NPs) in each of the samples and plotted the particle-size distribution.
As shown in the fitted curve, the particle-size distribution substantially conformed to the Gaussian distribution mode, and the particle-size distribution of the particles in each sample was narrow. The statistical chart also showed that the as-synthesized samples had a relatively uniform particle size, and as the VR added increased, the average particle size of the NPs also gradually increased from 1.57, 1.99, 2.03, 2.14 nm to 2.42 nm, respectively. On the other hand, in the case when the VR of the liquid NaK alloy remained constant with an excessive mole number over the stoichiometric precursor metal ions, the particle diameter of the alloy NPs also increased as the reaction time went on. We fixed VR at 160 μL, and changed the tR from 10 s, 30 s, 2 min, and 5 min to 10 min, respectively. We found the particle-size distribution of the samples was also in a narrow range, and the average sizes of the Pt–Cu NPs gradually increased as tR increased, with the sizes being 2.42, 2.5, 2.6, 2.7, and 3.2 nm, respectively. A three-dimensional map was plotted and is shown in Fig. 2j, in which the variation of the average sizes of the as-synthesized Pt–Cu NPs with VR and tR can be clearly observed. Meanwhile, another statistical curve in Fig. 2k shows that the average sizes of the samples synthesized using more reducing agent had a larger increase than the smaller ones as the reaction time went on. These results indicated that it was easy to control the synthesis of sub-3 nm alloy NPs by changing the amount of reducing agent and the reaction time at room temperature.
Fig. 3a and b further display the detailed morphology of the Pt–Cu NPs formed on vxc-72 through the TEM and HRTEM images, which clearly show the uniform and dense dispersion of Pt–Cu NPs on the surface of the carbon supports. The average particle diameter of the alloy NPs was about 3 nm. Also, essentially, there were no separate alloy particles that were not supported on the carbon, which demonstrated that heterogeneous nucleation in the reduction system is advantageous in the presence of a carbon support. Fig. 3b shows a high-resolution transmission electron microscope (HRTEM) image of the Pt–Cu alloy NPs. The interplanar spacing was measured as 0.22 nm, which corresponded well to the (111) plane of the Pt–Cu crystallite. The formation of the alloy and the elemental surface fraction can be disclosed by the elemental mapping images of Pt, Cu and C in Fig. 3d, e and S2 in the ESI.† As expected, Pt, Cu atoms were evenly distributed on the alloy particles. X-ray adsorption near edge structure (XANES) and extended X-ray adsorption fine structure (EXAFS) spectroscopy were performed for the PtCu/C sample and reference Pt foil. The Pt L3-edge XANES results of the PtCu/C and the Pt foil are shown in Fig. 3f. The white line intensities in the normalized XANES spectra reflect the oxidation state of Pt. As shown in Fig. 3f, the white line intensity of PtCu/C is lower than that of the Pt foil, revealing a decrease in the oxidation state of Pt within PtCu/C. Fig. 3g shows the R-space Pt K edge of PtCu/C and the Pt foil, respectively. It can be seen from the elemental distribution map and Pt L3 edge XAFS spectra that the reduction method we used successfully reduced the added precursor to the alloy NPs.
Further, a series of ex situ X-ray diffraction (XRD) and ex situ X-ray photoelectron spectra (XPS) measurements were performed on the Pt–Cu nanoalloys to track the changes of their structure, composition, and valence states during the different reaction conditions. Fig. 4a shows the XRD patterns of the Pt–Cu alloy NPs with a face-centered cubic (FCC) structure and a lattice constant greater than copper and less than platinum. The peak appearing at 26° is the (002) crystal plane of the carbon support.45 The peaks appearing at 41° and 47° correspond to the (111) and (200) crystal planes of the Pt–Cu alloy NPs, respectively.34 On the basis of the XRD data shown in Fig. 4a, a clear transformation feature of the crystal lattice of the Pt–Cu nanoalloys during the different reaction conditions can be seen. When the reaction time was short (tR = 10 s) and the amount of the NaK alloy added was low (VR = 10 and 20 μL), it is most likely that Cu existed predominantly in the metallic alloy state. While, with increasing the reducing agent or extending the reaction time, the XRD peaks were shifted to the low angle direction, but close to that of the Pt–Cu alloy, indicating the formation of the Pt–Cu alloys. There were no separate characteristic peaks corresponding to Pt and Cu in the sample, which reflected that the as-synthesized alloy NPs appeared to be atomically mixed Pt–Cu alloy phases.
Fig. 4b shows the XPS spectra of a series of Pt–Cu nanocrystals on carbon supports. The relatively strong two peaks at 72.9 and 76.3 eV correspond to the metal Pt0, and the weaker peaks are derived from Pt2+. As the reducing agent or the reaction time increased, Pt 4f was shifted to a lower binding energy (BE). Thus, the lower-energy shift of Pt 4f indicated the formation of Pt–Cu alloys, which was in agreement with the XRD results. Likewise, the peaking of the Cu 2p orbital with the two peaks at 932.6 and 952.5 eV correspond to zero-valent copper. The low-shifting tendency of the Cu 2p peak can be clearly seen in the left graph in Fig. 4b, which is consistent with the trend of variation of Pt 4f. This negative shift phenomenon may be caused by an initial state effect, for example, charge transfer from a metal to a carrier, due to the small particle size, lattice strain, and many atoms having electron defects.33,46
To prove the universality of our synthesized strategy, a series of binary Pt–M (M = Fe, Co, Ni) and ternary Pt–Cu–Fe nanoalloys were deposited on a carbon support (vxc72), and were noted as Pt–Cu-vxc72, Pt–Co-vxc72, Pt–Ni-vxc72, Pt–Fe-vxc72, and Pt–Cu–Fe-vxc72. Fig. S2f–h† show the HAADF-STEM images and the corresponding EDS maps of Pt–Co NPs. Fig. 4c presents the XRD patterns of a series of as-synthesized binary alloys, which had an FCC structure with a lattice parameter closer to that of platinum. After comparison with the standard XRD spectra of Fe, Co, and Ni, it was found that no single peak of the corresponding metal appeared in the sample, and so it can be judged that the synthesized sample contained substantially no single metal particles and these had formed an alloy.
The overall morphology of the ternary Pt–Cu–Fe-vxc72 sample synthesized by the same method (VR = 160 μL, tR = 2 min) is shown in Fig. 5. The as-produced ternary alloy NPs were uniformly grown on carbon black. Within the entire larger display range, a relatively uniform and good dispersibility of the nanoparticles were demonstrated and no obvious agglomeration was observed. All of these topographical features contribute to further improving the catalytic performance of the material. The inside illustration is an HRTEM image of a Pt–Cu–Fe NPs, from which the crystal lattice of the alloy particles can be clearly shown. It could be calculated that the interplanar spacing of the nanoparticles was 0.23 nm, which corresponded to the (111) crystal plane of the alloy. Fig. 5c–f present the elemental distribution of the sample, showing the distribution of the four elements Pt, Cu, Fe, and C. The three metal elements Pt, Cu, and Fe were distributed in the nanoparticles, which further proved that we had successfully synthesized the ternary alloy. The valence state of the metal in the Pt–Cu–Fe-vxc72 sample could be analyzed by XPS, as shown in Fig. S3.† The survey XPS spectrum showed that the Pt–Cu–Fe-vxc72 contained elements such as Pt, Cu, Fe, C, and O. Among these, the O element may be derived from the partial oxidation of the sample when it was placed in the air.33,47
![]() | ||
Fig. 5 TEM (a), HRTEM (b), BF-STEM (c), and HAADF-STEM (d) images and (e–h) the corresponding EDS elemental maps of Pt–Cu–Fe-vxc72. |
To prove the utility of the nanoalloys, the hydrogen evolution reaction (HER) performance of a series of Pt–Cu-vxc72 samples was performed and the results are shown in Fig. 6. The polarization curves were obtained in a 0.5 M sulfuric acid electrolyte at a sweep rate of 5 mV s−1 (Fig. 6a). It can be seen that the different reducing agents and reaction time factors had a great influence on the electrocatalytic HER performance. When the amount of the reducing agent added was 160 μL and the reaction time was 10 min, the best hydrogen evolution performance of Pt–Cu-vxc72 was obtained, that is, the overpotential was 17 mV at a current density of 10 mA cm−2. In addition, for a more intuitive comparison of the sample performance, we calculated the overpotential of each material at a current density of 10 mA cm−2 and prepared a columnar chart (Fig. 6c).
When the amount of the reducing agent was insufficient (10 μL) and the reaction time was short (10 s), the sample had poor HER performance, and the overpotential at a current density of 10 mA cm−2 was as high as 165 mV. Fig. S4† shows the HER stability of the sample in 0.5 M H2SO4 (160 μL 1 min). The Tafel slope of each sample can be obtained from Fig. 6c and d. It can be seen that the sample prepared by using 10 μL reducing agent and a reaction time of 10 s had a relatively poor performance, with the largest Tafel slope of about 68 mV dec−1. The best HER performance of the Pt–Cu-vxc72 sample (160 μL 10 min) had the smallest Tafel slope, about 22 mV dec−1.
The HER performances of Pt-based binary Pt–M (M = Fe, Co, Ni) alloys NPs grown on carbon supports are shown in Fig. 7a. The Pt–Co-vxc72 sample had the best catalytic performance with only 3 mV overpotential to achieve a current density of 10 mA cm−2 in these samples, which was better than Pt–Fe-vxc72 and Pt–Ni-vxc72. At a current density of 60 mA cm−2, Pt–Co-vxc72 required a minimum overpotential of 42 mV, followed by Pt–Ni-vxc72 at 56 mV, while Pt–Fe-vxc72 required the maximum overpotential (59 mV). The Tafel slopes corresponding to the three samples can be observed in Fig. 7b. The Pt–Co-vxc72 sample had the smallest Tafel slope with only 30 mV dec−1. The Tafel slope can reflect information about the reaction rate control steps, which can be used to analyze the kinetic factors of electrochemical reactions.20 Previous studies have shown that there are three main steps in the hydrogen evolution reaction in an acidic solution. The smaller Tafel slope indicated that in our synthetic samples, the HER process occurred via the Volmer–Heyrovsky mechanism.48 A small Tafel slope means that the current density increases rapidly with the increase of the overpotential, so it can be judged that Pt–Co-vxc72 had the best catalytic performance among the three. Although our synthetic carbon-supported binary alloys had excellent catalytic properties, their stability in acidic media was not satisfactory (Fig. S4†). Therefore, we added Fe(acac)3 as a precursor of iron during the synthesis, and synthesized ternary Pt–Cu–Fe nanoalloys.
Fig. 7c shows the polarization curve of Pt–Cu–Fe-vxc72 in 0.5 M H2SO4 electrolyte. Although the amount of noble metal platinum was further reduced by doping the iron precursor to form a ternary alloy, the catalyst still maintained large activity in the hydrogen evolution reaction. Only 6 mV overpotential was needed to reach a current density of 10 mA cm−2. A current density of 60 mA cm−2 could be achieved with an overpotential of 16 mV. In addition, Fig. 7d shows the I-T curve of the material tested in the same electrolyte at the overpotential of 32 V vs. RHE, indicating that the ternary alloy formed by the addition of iron had good stability in the acidic environment. The current density was maintained for 20 h without significant attenuation, indicating that the activity of the catalyst was well maintained.
Overall, the as-produced metallic alloys exhibited excellent electrocatalytic hydrogen evolution performance, which could be further demonstrated by the CV test and the ECSA values calculated in Fig. S5† and the comparison of the mass specific activity among the Pt/C, Pt–Cu-vxc72, and Pt–Cu–Fe-vxc72 samples in Fig. S6.† The reasons for the excellent electrocatalytic performance are as follows. The absence of a surfactant in the reaction allowed for intimate contact between the Pt–Cu nanocrystals and the carbon support, which facilitated the catalysis of charge transfer in the HER. The ultrafine alloy NPs grown on carbon supports with uniform dispersion and high surface exposure provided a high density of catalytically active sites. The dispersibility between the particles was relatively good, so that the surface of the alloy NPs could be sufficiently exposed, which was favorable for the improvement of the electrocatalytic performance.24
The synthetic technique also presents several advantages as follows. (I) The K (−2.925 V) and Na (−2.712 V) metals have more negative reduction potentials than most metals, which ensure that this method can create nanoalloys from nearly any metallic combination. Especially, the metallic alloys that are difficult to synthesize by conventional methods in aqueous solution can be synthesized in a non-aqueous strong reduction system by NaK alloy. (II) The particle size, composition as well as the final structure can be handily and effectively tuned by controlling the reaction conditions (shearing time and volume of the reducing agent), which benefits the observation and optimization of new nanocatalysts. The uniform alloying of the Pt atoms in the as-formed PtCu NPs is proved in Fig. S7.† The shearing force generated by the rotor accelerates the homogenization process of the reducing agent with the reaction precursor and the carrier carbon black, so that the reduction reaction can occur rapidly and uniformly throughout the reaction system. (III) The rapid (synthesis in tens of seconds), low energy cost (at room temperature), and scalable (through a shearing treatment) synthetic procedure could enable the highly efficient production of alloy NPs. (IV) Moreover, the synthesis process does not require the addition of a surfactant to inhibit the growth of crystal grains. Instead, a strong reducing agent is used to achieve a process of explosive nucleation in a very short period of time. After the addition of the reducing agent, the concentration of the atoms in the solution rises rapidly to reach the concentration of nucleation, which greatly shortens the nucleation time and ensures that the growth grain size of the nanocrystals tends to be uniform. Meanwhile, a general method for synthesizing alloy nanocrystals without a surfactant at room temperature was proposed, which paves the way for exploring the application of tuning the size and composition of alloy nanocrystals to obtain the desired properties. The SA-LMR method is universal and can synthesize a series of bimetallic catalysts easily and quickly. The utilization of the shear-assisted liquid metal reduction approach to obtain ultrafine alloy NPs opens up new avenues for designing highly efficient nanocatalysts. This method greatly improves the synthesis rate of this type of catalyst, and provides a prospect for large-scale mass production and industrialization.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0na00412j |
This journal is © The Royal Society of Chemistry 2020 |