Morteza Hassanpour Amiria,
Jonas Heidlera,
Ahmar Hasnaina,
Saleem Anwarab,
Hao Lua,
Klaus Müllena and
Kamal Asadi*a
aMax-Planck Institute for Polymer Research, Ackermannweg 10, 55128, Mainz, Germany. E-mail: asadi@mpip-mainz.mpg.de
bSchool of Chemical & Materials Engineering, National University of Sciences & Technology, Sector H-12, Islamabad, Pakistan
First published on 6th January 2020
Doping-free transfer of graphene produced by catalytic chemical vapor deposition (CVD) on copper foil, is still a technical challenge since unintentional doping of the transferred graphene layer yields an uncontrolled shift of Dirac point in graphene-based field-effect transistors (FETs). Typically, CVD graphene is released from the growth template by etching of the template, i.e. copper. During the etching process, ions adhere to the graphene layer resulting in unintentional doping. We demonstrate that washing a CVD graphene layer in an aqueous ammonia flow bath after etching copper, removes the majority of the unintentional dopants. FETs fabricated from graphene after washing in DI-water display a large scattering in Dirac bias with lowered mobility. In contrast, FETs from graphene that is washed in ammonia furnish better performance with high geometrically normalized mobility exceeding 2.4 × 104 cm2 V−1 s−1, balanced transport and a Dirac voltage near zero. We attribute the improved FET behavior to effective removal of the ions with a typical density of 4 × 1012 cm−2 from the graphene layer.
Graphene transfer is one of the critical issues in the fabrication of graphene FETs and their upscaling.8 Since FETs are sensitive interface devices, the presence of ions (or any ionic species) at the interface between the graphene layer and the gate dielectric leads to unintentional doping of the graphene layer, which drastically affects the electrical performance.9–11 As a result, the Dirac point shifts to voltages much larger than 0 V so that instead of an ideal ambipolar behavior, the graphene FET exhibits unbalanced electron/hole transport or even a seemingly unipolar behavior.
Herein, we demonstrate CVD-based graphene FETs with balanced ambipolar electron/hole transport. Towards that end, we have introduced an extra washing step of graphene in aqueous ammonia after etching away the copper.12,19 The FETs are fabricated using the conformal transfer technique.8 Ammonia effectively removes the majority of ions (nearly 4 × 1012 cm−2 dopants) that otherwise would unintentionally dope the graphene layer. The extra washing step also improves the mobility of the charge carriers and shifts the position of the Dirac point to biases close to zero volt. We attribute the improved FET behavior to effective removal of Cu2+ from the graphene layer, and quantify the density of ions.
The process flow for graphene transistor fabrication is schematically shown in Fig. 1a. CVD graphene (Graphenea) on Cu foil (25 μm thickness, 99.8%) is coated with PMMA (Aldrich). To minimize errors due to batch-to-batch variations, all the experiments presented here are conducted using graphene obtained from small cuts of the same Cu foil. PMMA is dissolved in toluene (Acros) with 10 wt%, and filtrated through 1 μm filters prior to spincoating (all materials are used as received). The thickness of the PMMA layer varies from 700 to 800 nm. The graphene layer on the uncoated surface of the copper foil is removed using an oxygen plasma. The Cu foil is etched in 1 molar aqueous bath of FeCl3 and the floating graphene/PMMA layer is thoroughly washed with DI water. The “ammonia” treatment is performed by placing the floated graphene/PMMA film in a continuous flow bath of NH3:DI-water (1 molar) for 30 min followed by a drying step at 40 °C for 12 hours in a vacuum oven at 10−1 mbar. Hereafter, we use w-graphene and a-graphene to refer to graphene that is washed in DI-water or aqueous ammonia flow bath, respectively. Subsequently, the graphene/PMMA layers are transferred to a pre-patterned Si-wafer using the conformal transfer technique. After evaporation of residual water, the PMMA layer is removed in a fresh acetone bath. Subsequently, the exposed transferred graphene is washed in a deionized water bath. The final cleaning processes are repeated several times to minimize the PMMA debris. We note optimizing the transfer process toward full removal of the PMMA layer or minimizing structural defects were beyond the scope of this work.
The pre-patterned substrates are fabricated on 6-inch Si wafers with 250 nm of thermally grown SiO2. The electrodes are fabricated by sputter deposition of Ti/Au (2 nm/150 nm), and patterned by conventional photolithography. The spacing between the source and drain electrode varies from 1 μm to 40 μm at a fixed channel width of 1000 μm, having a concentric geometry. A scanning electron microscopy (SEM) image of the transistor test structure is given in Fig. 1b. A The SiO2 surface is passivated with hexamethyldisilazane (HMDS) prior to conformal transfer of graphene/PMMA. The graphene transferred onto a pre-patterned substrate is inspected using SEM. Although the pre-patterned substrates have an uneven topography, the SEM image presented in Fig. 1c–d, provides evidence that the graphene morphology on the Au contact and the SiO2 layer are identical and extrinsic defects such as cracks or film discontinuities are absent. Importantly, the same morphologies are observed for both w- and a-graphene. Both graphene layers showed some PMMA debris. A typical atomic force (AFM) topography image for the a-graphene layer is shown in Fig. 1e. The same AFM images are obtained also for the w-graphene (not shown here). From both TEM and SEM images it is clear that washing the graphene layer in an ammonia flow bath does not harm the integrity of the graphene layer. Presence of the PMAA layer during the ammonia washing and transfer steps is helpful for the structural integrity of the graphene.
Optical microscopy and atomic force microscopy (AFM) (Nanoscope Dimension 3100 Bruker) were used to analyze the surface morphology of the transferred graphene films before and after ammonia treatment. X-ray photoelectron spectroscopy (XPS) was conducted with a Kratos Axis Ultra DLD spectrometer (Kratos, Manchester, England) using Kα excitation of an Al source with a photon energy of 1487 eV. The data was acquired in the hybrid mode with a beam spot size of 300 × 700 μm2 using a 0° take-off angle, defined as the angle between the surface normal and the axis of the analyzer lens. A charge neutralizer was used during spectra collection to compensate sample charging. Survey and detailed region XP spectra were collected by setting analyzer pass energy at 80 eV, C 1s and O 1s high-resolution spectra were collected with an analyzer pass energy of 20 eV. A neutralizer was always used during spectra collection. No X-ray damage was inferred to the sample during measurements. Atomic compositions were calculated by subtracting a linear background from the collected spectra with setting an analyzer pass energy at 80 eV. The peak areas were normalized by the manufacturer supplied sensitivity factors, and atomic compositions were calculated accordingly with CasaXPS software.
The sheet resistance of the graphene layer, before and after ammonia treatment is determined using a circular transfer line test method (CTLM), as detailed in ref. 8. The sheet resistance is obtained by forcing different constant currents (ranging from 1 μA to 100 μA), and measuring the voltage drop. In total 32 test structures are measured. The extracted sheet and contact resistances are constant for different current levels.
Metal/insulator/graphene/metal (MIS-) diodes are fabricated by deposition of Cr/Au (1 nm/50 nm) on to thoroughly cleaned glass substrates. After deposition of the graphene/PMMA layer on the substrates and subsequent drying, 100 nm of a Au top contact are evaporated through a shadow mask. The PMMA layer thickness was 700 to 800 nm. The capacitors had a device area of 0.16 mm2. For each case, 25 MIS-diodes are fabricated and the results are averaged. All electrical measurements were performed in high vacuum (10−6 mbar) using a Keithley 4200 semiconductor characterization system and a Keysight 4980 precision LCR meter.
First, the sheet resistance, Rsh, of the graphene layer after different washing processes are determined from the CTLM test structures.8 The Rsh for w-graphene amounts to 450 Ω □−1 and remains constant for different current levels whereas the a-graphene layer shows an increased Rsh of 500 Ω □−1. Observation of higher Rsh is due to the de-doping of the graphene layer.
Transfer characteristics of the FET fabricated with w-graphene is presented in Fig. 2. The w-graphene FET exhibit a large shift in Dirac voltage towards positive voltage, and an unbalanced transport leading to a “seemingly” unipolar p-type instead of an ambipolar-like behavior. Both observations indicate that the w-graphene layer is doped with positively charged ions. Presence of ions screens the gate bias and shifts the Dirac voltage to large positive voltages. Therefore, we attribute the unipolar characteristics of the w-graphene FET to unintentional doping of the graphene layer during the transfer process.13–16 This can be caused by copper, water or etchant (FeCl3 in our case) ions. A doping/de-doping mechanism will be discussed later.
To eliminate the troublesome unintentional doping, and recover ambipolarity in the graphene FETs, we have introduced an extra washing step in ammonia flow bath, right before transfer of graphene/PMMA layer onto the FET substrate. The FET transfer characteristics of the resulting a-graphene FET is presented in Fig. 2. Interestingly, the FET shows a shift of the Dirac voltage to a gate bias near zero volt, namely 1–2 V. Moreover, the transistor shows a nearly symmetric transfer curve. This indicates a balanced charge carrier concentration in the graphene layer, i.e. the Fermi level is near or at the Dirac point, which means that ions, or charged species are absent. It should be added both transistors presented in Fig. 2 are fabricated from the same batch of CVD graphene, coated with PMMA.
It has been recently demonstrated that using paraffin instead of PMMA for the graphene transfer yields four-fold increase in field-effect mobility, μFE, of the graphene layer.17 Since μFE is a device parameter that is affected by the geometrical parameter W/L (channel width/length). For a fair comparison, here use a normalized mobility, μn, which is the μFE multiplied by the geometrical parameter W/L:
The current in the a-graphene FET is lower than the one in the w-graphene FET. This indicates that the ammonia treatment de-dopes the graphene layer, and reduces the number of residual carrier in the graphene layer. We suggest a tentative de-doping mechanism as follows. Aqueous FeCl3 is a well-known etchant for copper, and a strong Lewis acid. The chloride plays an essential role in dissolving copper since Cl− is a strong complexing agent for Cu2+ ions. The etching reaction is written in a simplified form as:
2Fe3+ + Cu → 2Fe2+ + Cu2+ | (1) |
The Cu ions in the form of CuCl2 are soluble in water. As a result there can always be traces of Cl− or Cu2+ ions in w-graphene. The extra washing step of graphene in an ammonia flow bath is ideal to remove both ions. The NH3 molecules extract the residual Cl− ions from the graphene layer as ammonium chloride, which is soluble in water and is washed away. Furthermore, the Cu2+ ions form an ionic complex in water, namely hexaaquacopper(II) ion [Cu(H2O)6]2+. The ammonia acts simultaneously as ligand for the [Cu(H2O)6]2+ ions to form solid precipitates of the neutral complex according to the following reaction:
[Cu(H2O)6]2+ + 2NH3 → [Cu(H2O)4(OH)2] + 2NH42+ | (2) |
Therefore, the extra ammonia washing step would also remove Cu2+ ions that can potentially act as dopant.
To unambiguously demonstrate the presence of ions and further estimation of their surface concentration we have performed XPS measurement for the graphene layer before and after ammonia transfer. A closer up X-ray photoelectron spectra18 for C 1s, Cu 2p, Fe 2p and Cl 2p for both w- and a-graphene are presented in Fig. 3. The C 1s spectrum of the graphene does not change before and after ammonia treatment, indicating that ammonia does not attack the CC bonds. The Fe 2p spectra shows that washing the graphene layer with DI-water is sufficient to effectively remove Fe ions, as the XPS spectra does not show presence of Fe before and after ammonia flow bath treatment. The Cu 2p spectra clearly shows a weak signal near 930 eV, which could be assigned to Cu (2p3/2) electrons. After the ammonia washing step, the weak signal has disappeared in the background noise. Therefore, washing of the graphene in the ammonia flow bath has removed minute traces of Cu ions. The difference in XPS spectra is more pronounced for the Cl 2p survey of w- and a-graphene. While the a-graphene does not show presence of Cl, the w-graphene clearly shows a peak at ∼199–200 eV. The amount of Cl for the w-graphene and a-graphene is calculated, which amount to 0.27 ± 0.04% and 0.16 ± 0.04% respectively. Therefore using an ammonia flow bath treatment has effectively removed majority of the Cl ions.
Fig. 3 High-resolution C 1s, Fe 2p, Cu 2p, and Cl 2p XPS spectra for w-graphene (top) and a-graphene (bottom). For every graphene layers, three separate samples are measured. |
To estimate the concentration of ions, we have fabricated MIS-diodes. A constant DC bias of +10 V superimposed with an AC signal of 0.1 V with variable frequency is applied to the Au electrode contacting PMMA. The capacitance–frequency responses of the MIS-diodes are given in Fig. 4. MIS-diodes from w-graphene show a decreasing capacitance with increasing frequency. The capacitance at 100 Hz is 160 pF which reduces to 130 pF at 100 kHz. The reduction in capacitance is directly related to ion mobility, because at low frequencies, the ions can follow the changes in the electric field, while at high frequency they are static. In sharp contrast, the MIS-diodes fabricated with a-graphene possess a lower capacitance of ∼30 pF that does not vary with the excitation frequency. A constant capacitance over a large frequency range is a clear indication that ions are absent in the MIS-diode stack. Since both MIS-diodes have similar PMMA thickness, we can calculate the difference in the number of excess positive ions/charges in w-graphene by considering the capacitances measured at 100 kHz. Taking 130 and 30 pF for w- and a-graphene respectively, we have estimated an areal doping density of 3.9 × 1012 cm−2 for w-graphene. The doping density is nearly the same as the intrinsic carrier density in graphene. As a result, a nearly two fold increase in the current of the transistors is expected when we assume that the mobility remains constant. Interestingly, the currents at Vg = −20 V for the transistors presented in Fig. 2 differs by a factor of 2.
In summary, washing of the graphene layer after etching copper in ammonia flow bath is a crucial step to achieve FETs with balanced transfer characteristics and with zero Dirac voltage. The ammonia can effectively remove both chlorine and copper ions. We note that the PMMA transfer technique is not ideal for the realization of high quality graphene FETs. Therefore, upon combination of ammonia flow bath with more advanced transfer techniques, high performance CVD-graphene based FET are within reach.
This journal is © The Royal Society of Chemistry 2020 |