Xuekun Jin‡
a,
Fengjuan Chen‡*ab,
Dianzeng Jia*a,
Yali Caoa,
Haiming Duanb and
Mengqiu Longc
aKey Laboratory of Energy Materials Chemistry, Ministry of Education, Key Laboratory of Advanced Functional Materials, Autonomous Region, Institute of Applied Chemistry, Xinjiang University, Urumqi, Xinjiang 830046, China. E-mail: jdz0991@gmail.com
bSchool of Physics Science and Technology, Xinjiang University, Urumqi 830046, Xinjiang, PR China. E-mail: cfj2008meet@163.com
cHunan Key Laboratory of Super Micro-structure and Ultrafast Process, Central South University, Changsha 410083, China
First published on 27th January 2020
The introduction of noble metal nanoparticles to photocatalysts can effectively improve the separation efficiency of the photogenerated electron–holes. Therefore, noble metal/ZnS composites were synthesized using a low-temperature solid-phase chemical method with sodium borohydride as the reducing agent. The characterization results showed that the noble metal/ZnS composites have been successfully obtained and that the noble metals were distributed on the surface of ZnS. The catalytic results suggested that the composites exhibited improved activity after introduction of noble metals, which can be attributed to the rapid migration of carriers and the enhancement of the light absorption, mainly owing to the tight combination between the ZnS and noble metals and the plasmon resonance effect of the noble metals. The catalytic mechanism was explored by using photoluminescence spectroscopy, photocurrent spectra, valence band X-ray photoelectron spectroscopy (XPS-VB) spectra and capture agent experiments, and a possible mechanism was proposed. This work provides a new strategy for the high-volume synthesis of noble metal-based composite photocatalysts, which could be helpful for sustainable development.
It has been found that the catalytic activity of ZnS can be improved by means of depositing noble metals, compounding semiconductors, exploring new materials, and so forth.9–13 Among these techniques, depositing noble metals is an effective approach to enhance the activity. This is because noble metal nanoparticles have a good electrical conductivity and electron-trapping ability, and can act as an electron medium to generate resonance in an electric field caused by illumination, which is called the surface plasmon resonance effect (SPR), and the effect can promote effective separation of the electron–hole.14–18 For example, Ayodhya et al. synthesized ZnxAg1−xS composites using the hydrothermal method, and the photocatalytic results showed that the composites exhibited an excellent photocatalytic degradation activity to organophosphorus pesticides after the introduction of Ag.19 The enhanced performance may be due to the plasmon resonance effect which causes the photogenerated electrons on the ZnS conduction band to be injected into the Ag surface, thereby promoting the efficient separation of the photogenerated carriers.20 Thus, depositing noble metals has been considered to be an effective strategy to enhance the photocatalytic properties.
In general, the composition, structure and properties of materials are closely related to their catalytic properties. It has been found that there are many methods for fabricating noble metal/sulfide composites, such as the microwave assisted reduction method, the photoreduction coupled water bath method, and the in situ deposition method.21–26 However, the above mentioned methods have some disadvantages, such as a complicated operation, high cost, and can be difficult to control. Therefore, it is highly desirable to find a simple and fast technique to obtain noble metal/sulfide composites. At present, our group has synthesized a series of nanomaterials with excellent photoelectric properties by using the low-temperature solid-phase chemical method.27–30 However, through consulting numerous studies, it has been found that the synthesis of noble metals/sulfides composites using this method have not been reported so far.
In this paper, Ag/ZnS composites and Au/ZnS composites were synthesized using a low-temperature solid-phase chemical method with the aid of the reducing agent sodium borohydride (NaBH4). The photocatalytic activity of the composites was studied by degrading methyl orange (MO) under UV light, and the photocatalytic mechanism was further discussed. It was found that the noble metal nanoparticles in the composites synthesized using the method have strong binding with ZnS, which facilitates the rapid separation of the photogenerated carriers and improves the catalytic activity.
In order to further study the influence of noble metals on the composition, structure and performance of ZnS, Au/ZnS composites were also synthesized under the same conditions as those described above. The difference was that AgCH3COO (0.0015 g) was replaced with AuCl·HCl·4H2O (0.021 g, the mass percentage of Au and ZnS was 0.1), and the Au/ZnS composite was obtained and designed as AUZS-0.1. By changing the mass percentage of Au and ZnS, composites AUZS-0.2, AUZS-0.5, AUZS-1, AUZS-2 and AUZS-5 with different compositions were also prepared.
For the convenience of comparison, pure ZnS was also synthesized without NaBH4, AgCH3COO and AuCl·HCl·4H2O.
The procedure was performed as follows: 25 mg catalyst was added to 50 mL MO solution (10 mg L−1). In order to reach the adsorption equilibrium between the catalyst and MO solution, the adsorption was allowed to progress for 2 h under dark conditions. Subsequently, the light source was turned on for testing. 3.5 mL of the reaction solution was taken at intervals of 20 min, centrifuged at a certain speed (rotation speed of 10000 rpm) for 10 min, and the supernatant was taken and analyzed for the concentration of MO. The concentration of MO was measured using an UV-vis spectrometer with a range of 300–700 nm.
In order to study the active substances in the catalytic process, a capture agent experiment was carried out. The capture agents adopted were EDTA-Na2, ethanol and 1,4-benzoquinone. The experimental procedure was the same as that described above, except that a certain amount of capture agent was added to the system.
In order to clearly observe the morphology of the samples, transmission electron microscopy (TEM) analyses were conducted as shown in Fig. 2. It can be seen that the ZnS nanoparticle with a size of about 50 nm, has a slight agglomeration (Fig. 2a). In Fig. 2b, as for the composites AGZS-2, a small amount of Ag nanoparticles are present on the surface of ZnS. To further study the structure of the composites, high-resolution transmission electron microscopy (HRTEM) analysis was performed. In Fig. 2c, the composite AGZS-2 has clear lattice fringes, in which the lattice spacing of 0.30 nm corresponds to the (111) crystal plane of cubic ZnS, and the lattice spacing of 0.24 nm is consistent with the (111) crystal plane of the cubic Ag, suggesting the presence of the ZnS and Ag phases in the region.33 At the same time, there is a clear boundary between the ZnS and Ag lattices, indicating the formation of Ag/ZnS composites. In addition, the SAED results (Fig. 2d) indicate that the composites have a polycrystalline property.
Fig. 2 TEM images of ZnS (a), Ag/ZnS composite AGZS-2 (b); HRTEM image (c), and SAED patterns of the composites AGZS-2 (d). |
Specific surface areas on the Ag/ZnS composites were also characterized using nitrogen (N2) adsorption–desorption. As shown in Fig. S1,† the Ag/ZnS composites all display a typical type IV isotherm with a distinct hysteresis loop. The BET specific surface area of the Ag/ZnS composites AGZS-0.1, AGZS-0.2, AGZS-0.5, AGZS-1, AGZS-2 and AGZS-5 are 38.85, 48.31, 60.04, 72.36, 239.83 and 53.01 m2 g−1, respectively. When the mass percentage of Ag to ZnS is two, the composite AGZS-2 exhibited the largest specific surface area in comparison with the others, which is helpful for the adsorption and carrier transport, and the composite AGZS-2 displayed the highest photocatalytic activity (as shown in Fig. 5a).
The chemical composition of pure ZnS and the composite AGZS-2 was studied using an XPS technique. In the survey spectra (Fig. 3a), characteristic peaks for S 2p, C 1s, Ag 3d, O 1s, and Zn 2p appear, in which C 1s and O 1s are derived from the test process,34 confirming the presence of the S and Zn elements for ZnS, and the presence of the S, Ag and Zn elements in the compositeAGZS-2. Pure ZnS exhibits characteristic peaks of S 2p3/2 and S 2p1/2 orbitals at 161.6 and 162.6 eV (Fig. 3b), respectively, indicating the existence of the S element.35 In contrast, the characteristic peaks of the S element in composite AGZS-2 were slightly red-shifted to 161.7 and 162.8 eV, respectively. In Fig. 3c, the pure ZnS exhibits characteristic peaks of Zn 2p3/2 and Zn 2p1/2 orbitals at 1021.9 and 1044.9 eV, respectively. However, there is a slight red shift for the Zn 2p characteristic peaks in the composites AGZS-2, suggesting that there are interactions between Ag and ZnS.36 The characteristic peaks at 368.0 and 373.9 eV in Fig. 3d correspond to the Ag 3d5/2 and Ag 3d3/2 orbitals of metallic Ag, respectively, indicating the presence of the Ag element in the composite AGZS-2.37 The above described results show that there is ZnS and Ag in the composites, that is, the Ag/ZnS composite photocatalyst is obtained. XPS analysis was further performed to measure the Ag percentage in the Ag/ZnS composites. The Ag percentage with respect to ZnS was found to be 1.5% in the composite AGZS-2, which further proved the expected Ag percentage in the ZnS.
Fig. 3 XPS spectra of the ZnS and Ag/ZnS composites AGZS-2 (a) survey; (b) S 2p; (c) Zn 2p; and (d) Ag 3d. |
The optical absorption properties of the ZnS and Ag/ZnS composites were studied as shown in Fig. 4. It can be found that pure ZnS has an absorption in the range of 250–400 nm, which is consistent with the literature.38 After introducing Ag, Ag/ZnS composites showed a slight blue shift, which may be due to its small size (Fig. 4a). At the same time, with the formation of Ag/ZnS composites, a new absorption band appeared in the range of 450–800 nm, which is caused by the SPR effect of Ag, further indicating the presence of Ag.39 As the amount of Ag increases, the absorption capacity increases continuously, indicating that the composites will exhibit improved photocatalytic activity.
According to the Tauc equation αhν = A(hν − Eg)n,40 the band gap energy of the samples can be estimated by plotting the photon energy (hν) by (αhν)1/2, as shown in Fig. 4b. It can be seen that the band gap energies (Eg) of ZnS, the Ag/ZnS composites AGZS-0.1, AGZS-0.2, AGZS-0.5, AGZS-1, AGZS-2, and AGZS-5 are 3.38, 3.52, 3.49, 3.47, 3.46, 3.43 and 3.44 eV, respectively. It can be seen that with the increase in the Ag content, the band gap of the Ag/ZnS composites decreases first and then increases. Furthermore, the Eg of composite AGZS-2 is the smallest, which may be related to its structure and properties.
Fig. 5 (a) Photocatalytic performance of the ZnS and Ag/ZnS composites in the degradation of MO under UV light; and (b) the kinetic curve. |
Fig. 5b shows the kinetic results for the ZnS and Ag/ZnS composites. It can be seen that the photocatalytic degradation of MO complies with a quasi-first-order kinetic reaction.42 The rate constants of pure ZnS and composite AGZS-2 were 0.00193 and 0.00581 min−1, respectively. Compared with pure ZnS, the degradation activity of composite AGZS-2 increased by three times, indicating that the composites exhibit excellent photocatalytic activities. Furthermore, the recycling activity of the Ag/ZnS composites has been tested, and we found that the stability is relatively high (Fig. S2†).
In order to study the photocatalytic mechanism of the Ag/ZnS composites, the photocurrent response, photoluminescence (PL) spectra, capture agents and valence band XPS (XPS-VB) spectra measurements were conducted, as shown in Fig. 6.
From Fig. 6a, it can be seen that the pure ZnS exhibits a relatively low photocurrent response. After the introduction of Ag, the Ag/ZnS composites displayed a significantly increased photocurrent higher than that of ZnS. In particular, the composite AGZS-2 showed the strongest photocurrent signal, indicating that there is an efficient electron transfer between ZnS and Ag. Hence, the introduction of Ag can effectively improve the separation efficiency of the photogenerated electron–holes and exhibit an enhanced activity, which can also be verified by the photocatalytic results (Fig. 5).43
Fig. 6b shows the PL spectra of the pure ZnS and Ag/ZnS composites. The PL intensities of the composites significantly decreased after introducing Ag. Among them, the composite AGZS-2 exhibited the lowest PL intensity, indicating that introducing Ag can effectively inhibit the photogenerated charge recombination and further improve the photocatalytic activity.44
The role of active components in the catalytic process was investigated using a capture agent experiment. Here, disodium edetate (EDTA-Na2), ethanol (ethanol) and p-benzoquinone (1,4-benzoquinone) were used as capture agents of holes (h+), hydroxyl radicals (·OH) and superoxide radicals (·O2−), respectively.45 The degradation curves of MO after adding the above capture agents are shown in Fig. 6c. When EDTA-Na2 was added, the degradation rate to MO by the composite AGZS-2 is obviously improved, indicating that h+ is not an active component that affects the degradation process of MO. The degradation efficiency was inhibited to some extent after ethanol was added, indicating that ·OH is one of the active components, but is not the main component. When 1,4-benzoquinone was added to the reaction system, the degradation rate was significantly reduced, indicating that ·O2− is the main active component during MO degradation. It can be seen that ·O2− is the main active species that affects MO degradation, and ·OH is the second.
The position of the band determines the redox capacity of the photogenerated carriers during the catalytic degradation process. Therefore, XPS-VB spectra measurements of ZnS and composites AGZS-2 were performed, and the results are shown in Fig. 6d. The valence band edge (EVB) of ZnS and composite AGZS-2 are 0.49 and 0.96 eV, respectively, wherein the potential of the valence band of composite AGZS-2 is higher than that of ZnS (0.49 eV). This indicates that composite AGZS-2 has a stronger oxidizing power and catalytic activity than that of pure ZnS, probably due to the presence of Ag. Combined with the UV-vis results, the Eg values of the ZnS and composite AGZS-2 are 3.38 and 3.43 eV, respectively. According to the formula Eg = EVB − ECB, the determined conduction band edge (ECB) values of the ZnS and composite AGZS-2 are −2.89 and −2.47 eV, respectively.
As for composite AUZS-2, the Au nanoparticles at about 20 nm are distributed on the surface of ZnS (Fig. 8a). While, in Fig. 8b, the crystal plane distances of 0.31 and 0.26 nm correspond to the (111) plane of ZnS and the (111) plane of Au, respectively.47 This is in agreement with the XRD results, demonstrating the successful synthesis of the Au/ZnS composites. The SAED pattern in the inset further indicates the polycrystalline properties of the composites.
The survey spectrum (Fig. 9a) confirmed that there are S, Zn and Au elements in the composite AUZS-2. In Fig. 9b, the characteristic peaks of the S 2p3/2 and S 2p1/2 orbitals of the composite AUZS-2 are slightly red-shifted to 161.9 and 162.8 eV compared to the pure ZnS, respectively, suggesting there are interactions between Au and ZnS. As for the composite AUZS-2, characteristic peaks for the Zn 2p3/2 and Zn 2p1/2 orbitals appear at 1021.8 and 1044.8 eV, respectively (Fig. 9c). The two peaks for Au 4f5/2 at 88.7 and 91.6 eV are assigned to Au0 and Au1+, respectively (Fig. 9d), indicating the presence of the Au element in composite AUZS-2.48 The above described results show that there are two phases of ZnS and Au in the composites, that is, the Au/ZnS composites are obtained. From the XPS analysis, it can be found that the Au percentage with respect to ZnS was 1.9% in the composite AUZS-2, in agreement with the expected results.
After the introduction of Au, the Au/ZnS composites have a significant blue shift compared with that of ZnS (Fig. 10a). At the same time, with the formation of the Au/ZnS composites, a new absorption band appears in the range of 450–800 nm, which is caused by the plasmon resonance effect of Au, indicating the presence of Au in the composites.49 According to the Tauc equation αhν = A(hν − Eg)n, the Eg of the Au/ZnS composites AUZS-0.1, AUZS-0.2, AUZS-0.5, AUZS-1, AUZS-2, and AUZS-5 are 3.38, 3.57, 3.53, 3.54, 3.57, 3.55 and 3.59 eV, respectively (Fig. 10b). It can be seen that the Eg of composite AUZS-2 is relatively small, which may be related to the structure and properties.
The photocatalytic activity of the Au/ZnS composites were also explored as shown in Fig. 11. As the amount of Au increases, the photocatalytic activity of the Au/ZnS composites first increases and then decreases (Fig. 11a). When the mass percentage of Au to ZnS is two, the composite AUZS-2 exhibited the highest photocatalytic performance. The enhancement of the photocatalytic ability can be ascribed to the close combination of Au and ZnS and the SPR effect of Au, which facilitates the rapid separation of photogenerated carriers and thus improves the catalytic performance.50
Fig. 11 (a) Photocatalytic performance of ZnS and Au/ZnS composites for the degradation of MO under UV light, and (b) the kinetic curve. |
In order to compare the photocatalytic activities of the Au/ZnS composites and Ag/ZnS composites, Fig. S3† was examined. It can be found that 44% of MO was degraded by the Au/ZnS composite AUZS-2 after irradiation for 120 min, lower than that of the Ag/ZnS composite AGZS-2 (49%), indicating that the Ag/ZnS composites possess a higher photocatalytic activity than that of the Au/ZnS composites.
Fig. 11b indicates that the Au/ZnS composite photocatalytic degradation of MO conforms to a quasi-first-order kinetic process. The rate constant of the composite AUZS-2 was 0.00471 min−1, three times higher than that of ZnS, indicating that the Au/ZnS composite exhibits an excellent photocatalytic performance after introducing Au. In addition, we can see that the Au/ZnS composites also exhibited a stable photocatalytic activity (Fig. S4†).
Subsequently, the photocatalytic mechanism of the Au/ZnS composites was further studied as shown in Fig. 12. In Fig. 12a, the photocurrent of the Au/ZnS composites increases significantly after introduction of Au, and composite AUZS-2 exhibits the strongest photocurrent signal, indicating that introducing Au can effectively improve the separation efficiency of the photogenerated charges.51 In Fig. 12b, the PL intensity of the composites significantly decreased after introducing Au. Wherein the composite AUZS-2 displayed the lowest PL intensity, implying an excellent separation ability of photogenerated charges, which was consistent with the results of the photocurrent analysis (Fig. 12a).52 The results of the capture agent experiment (Fig. 12c) indicate that ·O2− is the main active substance, followed by ·OH. In addition, a XPS-VB spectrum study was performed on composite AUZS-2, as shown in Fig. 12d. The determined EVB of composite AUZS-2 is 1.31 eV, which is higher than that of ZnS (0.56 eV), indicating that composite AUZS-2 has a strong oxidizing ability.53 Combined with UV-vis results, the Eg of the composite AUZS-2 was found to be 3.55 eV. According to the formula Eg = EVB − ECB, it can be determined that the ECB of composite AUZS-2 is −2.24 eV.
Here, we take the Ag/ZnS composite as an example. First, the improved catalytic activity of the Ag/ZnS composites is mainly due to the rapid generation and migration of photogenerated charges. According to the results of the above mentioned UV-vis and XPS-VB tests, the ECB and the EVB position of ZnS are −2.89 and 0.49 eV, respectively. According to the literature, the Fermi level of Ag is located at 0.4 eV (vs. a normal hydrogen electrode (NHE)).54 Under UV irradiation, ZnS is excited and generates electron–hole pairs. Driven by the difference in the ZnS conduction band potential and the Ag Fermi level potential, photogenerated electrons of ZnS will rapidly migrate to the Ag surface, effectively reducing the recombination of the photogenerated electrons and holes on the surface of ZnS, which can also be confirmed by the results of the photocurrent and PL spectra (Fig. 6). However, when the mass percentage of Ag to ZnS increases to five, a new carrier recombination center is generated, thereby reducing the catalytic activity of the Ag/ZnS composites.
Secondly, the active species involved in the reaction is the direct cause of the enhanced photocatalytic activity of the Ag/ZnS composites. After photogenerated electron–hole separation, it is further converted into an active species (·OH, h+, ·O2−) to complete the degradation of MO. As can be seen from Fig. 13, the valence band position of ZnS (0.99 eV) is higher than the OH−/·OH potential (1.99 V vs. NHE). Therefore, ·OH (eqn (1)) cannot be obtained by oxidizing OH−. However, ·OH appears in the Ag/ZnS composites as shown in Fig. 6c. This may be due to the fact that after introduction of Ag, the reaction time of the electron is increased, and then a multi-electron reaction with oxygen occurs, indirectly generating ·OH (eqn (2)).55 In addition, as the photogenerated electrons aggregate on the Ag nanoparticles, the Fermi level increases and is higher than the O2/·O2− potential (−0.046 V vs. NHE), and then the electron can reduce O2 to ·O2− (eqn (3)). The same conclusion can also be obtained in the degradation of MO by the Au/ZnS composites.
OH + hVB+ →·OH | (1) |
O2 + 2H+ + 3eCB → OH− +·OH | (2) |
O2 + eCB →·O2− | (3) |
In summary, the mechanism of the catalytic degradation of MO by noble metal/ZnS composites can be briefly described as follows. Under UV irradiation, photogenerated electrons and holes are generated on the surface of ZnS, and electrons rapidly migrate to noble metal nanoparticles, thereby achieving the effective separation of electrons and holes on the surface of ZnS. Next, electrons on the noble metal nanoparticles react with O2 to obtain the active species ·O2− and ·OH. Eventually, the active species react with MO and then converts it to H2O and CO2, thereby achieving the degradation of MO.
Footnotes |
† Electronic supplementary information (ESI) available: Fig. S1 shows the N2 adsorption–desorption isotherms for the Ag/ZnS composites. Fig. S2 exhibits the recycling activity of the Ag/ZnS composite AGZS-2. Fig. S3 displays a comparison of the photocatalytic activities between the Ag/ZnS composites and Au/ZnS composites. Fig. S4 shows the recycling activity of the Au/ZnS composite AUZS-2. See DOI: 10.1039/c9ra07163f |
‡ These authors contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2020 |