Dandan Yan‡
,
Tingting Wei‡,
Wencheng Fang,
Zhanbin Jin,
Fengyan Li*,
Zhinan Xia and
Lin Xu*
Key Laboratory of Polyoxometalate Science of Ministry of Education, Department of Chemistry, Northeast Normal University, Changchun, Jilin 130024, P. R. China. E-mail: lify525@nenu.edu.cn; linxu@nenu.edu.cn; Fax: +86-0431-85099765; Tel: +86-0431-85098760
First published on 3rd September 2020
Recently, TaON has become a promising photoelectrode material in the photocatalytic field owing to its suitable band gap and superior charge carrier transfer ability. In this work, we prepared a TaON/CdS photocatalytic film using a CdS nanoparticle-modified TaON film by the successive ionic layer adsorption and reaction (SILAR) method. For the first time, the ZnS nanoparticles were deposited on the TaON/CdS film using the same method. We found that pure TaON had a nanoporous morphology, thus resulting in high specific surface area and better gas adsorption capacity. Furthermore, the TaON/CdS/ZnS film displayed a highly efficient NO2 photodegradation rate under visible light irradiation owing to its stronger visible light response, photocorrosion preventive capacity, and the high separation efficiency of photo-induced electrons and holes. Interestingly, the promising TaON/CdS/ZnS film also possessed remarkable recyclability for NO2 degradation. Therefore, we suggest that the TaON/CdS/ZnS photocatalytic film might be used for the photocatalytic degradation of other pollutants or in other applications. We also put forward the feasible NO2 photocatalytic degradation mechanism for the TaON/CdS/ZnS film. From the schematic diagram, we could further obtain the photo-generated carrier transport process and NO2 photodegradation principle in detail over the ternary photocatalytic film. Moreover, the trapping experiment demonstrates that ·O2− and h+ all play significant roles in NO2 degradation under visible light irradiation.
In the past few years, TaON has gradually become one of the most promising and highly regarded photocatalytic materials due to its suitable bandgap (about 2.5 eV) and positions of the valence band and conduction band, and its environmentally friendly features.20,21 Being yellow, yellow-green and orange-yellow in color, TaON can absorb visible light, thus turning into a relatively new and interesting photocatalyst.22,23 As such, TaON used to be a quite important and popular photocatalyst for solar water splitting (water splitting into H2 and O2).24–28 Nevertheless, further extensive applications of pure TaON material are limited, to some extent benefiting from its recombination losses of photogenerated electron and hole pairs, self-oxidative deactivation, low carrier mobility and poor stability.29,30 The construction of heterogeneous materials could well facilitate electron transportation and charge separation, thus improving the photoelectrochemical performance, e.g., SnO2/SnS2, SnO2/C, MoS2/C, etc., as previously reported.31–33 Accordingly, some researchers have worked out some composite materials and heterojunctions of TaON to overcome these drawbacks to further modify and enhance the photocatalytic performance.34–36 Recently, apart from the photocatalytic decomposition of water, the TaON material family has also been used for the photocatalytic degradation of pollutants and has served as the counter electrode for dye-sensitized solar cells.37,38 To date, using TaON photocatalysts to eliminate NO2 has not been investigated and we have found that TaON could be a good photocatalyst for NO2 photodegradation due to its nanoporous morphology and effective response to visible light.
Plenty of other semiconductors have been used to modify TaON material in order to further strengthen its photoelectrochemical performance. Among them, CdS, possessing a relatively narrow bandgap (approximately 2.4 eV) and a more negative conduction band position leading to its excellent responsiveness to visible light, is one of the most attractive photocatalytic materials.39,40 Various methods, such as chemical bath deposition (CBD), successive ionic layer adsorption and reaction (SILAR) and electrochemical deposition have been investigated to assemble CdS on some semiconductor material film.41–44 Unfortunately, the photocatalysts modified by only CdS hardly presented enhanced photocatalytic activity, which is because CdS is prone to photo-corrosion during photocatalysis, in other words, because S2− is easily oxidized by photo-induced holes.45 Therefore, some useful strategies have been explored to overcome this fatal disadvantage of CdS. Building heterostructures and loading co-catalysts are the widely adopted strategies.46 Employing ZnS as the passivation layer to effectively prevent the photo-corrosion of CdS is the broadest and most effective method. For instance, structures like CdS/ZnS nanoparticle composites, CdS–ZnS core–shell structures and core/shell CdSe/ZnS QDs, etc. have been established to achieve enhanced photostability and photocatalytic ability.47–51 Zhu's group prepared CdS@TaON core–shell composites coupled with graphene oxide nanosheets and Hou's group fabricated MoS2–CdS–TaON hollow composites, which have all achieved efficient photocatalytic hydrogen production.52,53 Zhang's group synthesized ZnS–CdS–TaON nanocomposites through a modified sol–gel method for photocatalytic hydrogen evolution.54 However, the preparation methods of TaON and ZnS–CdS–TaON are cumbersome and result in different morphologies and different photocatalytic properties.
Here, we have successfully prepared such photocatalytic films containing pure TaON, TaON/CdS and TaON/CdS/ZnS films through simple and effective methods (successive ionic layer adsorption and reaction (SILAR) method) to study their photoelectrochemical performances. We have carried out a series of experiments on the photocatalytic degradation of NO2 under visible light irradiation to check the photocatalytic capacities of these fabricated films. We found that photoelectrochemical tests, as well as NO2 degradation measurements, confirmed that TaON/CdS with the ZnS passivation layer exhibited the best charge carrier separation rate, most outstanding photocatalytic activity and excellent stability for NO2 photodegradation. The TaON/CdS/ZnS film exhibited remarkably increased NO2 degradation efficiency as compared to the pure TaON film, which achieved 96.7% in 2 h. Finally, we designed a schematic diagram of possible photocatalytic degradation mechanisms to investigate, in-depth, the reasons for the significant improvement in the photocatalytic performance of the TaON/CdS/ZnS photocatalytic film. The trapping experiment over TaON/CdS/ZnS film was conducted to further study the main active species in NO2 photodegradation.
The simple schematic diagram for the NO2 photodegradation system exhibited in Fig. S1† enables us to understand the photocatalytic degradation process. About 800 ppb of NO2 was first infused into a 500 mL quartz reaction vessel containing the photocatalytic films, and the system was kept in the dark for 30 min at room temperature to reach the adsorption–desorption equilibrium. Afterwards, 2.5 mL of gas was sucked from the system and transfused into the absorption liquid, and the absorbance served as the initial concentration (C0). The vessel was then irradiated with visible light for 0.5 h, 1 h, 1.5 h and 2 h, respectively. After irradiation, 2.5 mL gas was taken out and injected into the absorption liquid and the absorbance was used as the final concentration (C). Therefore, (C0 − C)/C0 ×100% was used to calculate the NO2 degradation efficiency.
The cycling experiment of NO2 photodegradation over TaON/CdS/ZnS film was conducted as follows. The ternary composite film was first used for NO2 photodegradation with visible light illumination for 2 h. The film was kept in air for 1 h and then used to again photocatalytically degrade NO2 for 2 h. This procedure was repeated 4 times to determine the recyclability and stability of the TaON/CdS/ZnS photocatalytic film.
The SEM morphologies and photographs of TaON, TaON/CdS and TaON/CdS/ZnS films are shown in Fig. 2. The porous microspheres possess a relatively irregular particle profile with a large number of nanopores (Fig. 2a and b). The CdS particles were uniformly deposited on TaON films with plenty of nanopores (Fig. 2c). The nanopores were completely covered after depositing ZnS particles onto the TaON/CdS films (Fig. 2d). The uniform microspheres did not change with the deposition of CdS particles or CdS and ZnS particles. The EDX analyses of pure TaON, TaON/CdS and TaON/CdS/ZnS photocatalysts are exhibited in Fig. S2,† which fully illustrates the presence of all the elements they contained. Fig. S3† shows the corresponding EDX element mappings of TaON/CdS/ZnS films. It was found that all the elements containing Ta, O, N, Cd, Zn and S were distributed uniformly throughout the TaON/CdS/ZnS composite film, which powerfully confirmed the even co-deposition of CdS and ZnS on TaON films.
To further prove the structure of all films, the measurements of N2 adsorption–desorption isotherms and the corresponding PSD were conducted and displayed in Fig. S4.†
The films showed a type IV isotherm with a type H3 hysteresis loop, suggesting the presence of mesopores. Fig. S4† reveals that the BET surface area of TaON was 47.56 m2 g−1, which was bigger as compared to TaON/CdS (6.12 m2 g−1) and TaON/CdS/ZnS (4.93 m2 g−1). This result may be due to the deposition of CdS and ZnS. Table S1† shows that the pore sizes of all films were in the range of 2–50 nm, indicating the mesoporous structure, which resulted in enhanced harvesting of the visible light.56,57 Compared to pure TaON, TaON/CdS and TaON/CdS/ZnS films demonstrated a hierarchical porosity composed of macropores and mesopores, and this interesting porosity facilitated fast mass transport, thus resulting in improved photocatalytic activity.58–60
The purpose of TEM performance was to further determine the microstructure of the TaON/CdS/ZnS composite films. As shown in Fig. 3a, the TaON/CdS/ZnS film exhibited an inconspicuous particle profile with a rough surface and lots of small-sized of CdS and ZnS particles were homogeneously dispersed on the TaON surface. To further confirm the existence and the specific locations of CdS and ZnS particles in the composite film, HRTEM analysis was conducted which is illustrated in Fig. 3b. The region with an interplanar spacing of 0.273 nm is consistent with the (111) crystallographic plane of the monoclinic-phase TaON. This observation corresponds to the XRD results. At the interface of CdS and TaON, the HRTEM image showed a lattice fringe spacing of 0.336 nm in accordance with the (111) plane of CdS. The lattice spacing of 0.308 nm was assigned to the (111) plane of ZnS at the edge of the composite film.54 Therefore, the TEM and HRTEM analyses amply demonstrated the co-existence and the position of CdS and ZnS in the TaON/CdS/ZnS film.
Fig. 4 displays the UV-vis absorption spectra to better assess the light-harvesting abilities of the as-fabricated TaON, TaON/CdS and TaON/CdS/ZnS photocatalyst thin films. The characteristic absorption edge at the near-infrared area was observed for pure TaON, probably due to the orange-colored TaON powder, implying that the pure TaON film possesses the excellent ability to absorb visible light. This result was consistent with the charge transfer process from the valence band to the conduction band of the TaON photocatalyst film under visible light irradiation. For the TaON/CdS and TaON/CdS/ZnS films, although the absorption edges at around 650 nm demonstrated a blue shift, the light absorption intensity exhibited obvious enhancement at 400–540 nm as compared to the pure TaON. The TaON/CdS/ZnS film showed a more significant increase than TaON, fully exhibiting the stronger absorption capacity and more excellent photocatalytic activity after depositing CdS nanoparticles on the TaON film and with the ZnS-passivation layers at the same time.
Fig. 4 UV-vis absorption spectra of the as-prepared TaON, TaON/CdS and TaON/CdS/ZnS films, respectively. |
To verify the specific surface chemical constituents and elemental valencies of the as-synthesized TaON/CdS/ZnS photocatalyst film, XPS spectra were studied and the C (1s) peak at 284.8 eV served as the reference peak to calibrate the XPS spectra. From the XPS survey spectra in Fig. S5,† Ta, O, N, Cd, Zn and S elements were all detected in the prepared composite sample, corresponding to the chemical compositions of TaON/CdS/ZnS. In Fig. 5a, two peaks at 25.7 eV and 27.5 eV were attributed to 4f7/2 and Ta 4f5/2 signals, respectively, consistent with the +5-oxidation state of Ta.61 The binding energy of N 1s was 404.7 eV, indicating the existence of the −3-oxidation state of N (Fig. 5b). Fig. 5c presents the peak at 532.0 eV, assigned to the O 1s, which corresponds to O2−.54 The binding energies of 404.9 eV and 411.7 eV in Fig. 5d were ascribed to Cd 3d5/2 and Cd 3d3/2, which belonged to Cd2+. As shown in Fig. 5e, two symmetric peaks at 1021.6 eV and 1044.7 eV belong to Zn 2p1/2 and Zn 2p3/2, corresponding to the state mainly reported for divalent sulfides. In Fig. 5f, S 2p can be divided into two peaks 2p3/2 and 2p1/2, located at 160.1 eV and 161.5 eV, respectively. This result demonstrated that the Cd–S and Zn–S bonding existed in the TaON/CdS/ZnS photocatalytic film.46
Fig. 5 XPS spectra of (a) Ta 4f, (b) N 1s, (c) O 1s, (d) Cd 3d, (e) Zn 2p and (f) S 2p for the TaON/CdS/ZnS composite film. |
The transfer, separation and trapping of photogenerated charge carriers on the as-fabricated film surfaces were determined via photoluminescence spectroscopy (PL) and the typical photoexcitation wavelength was 400 nm, as exhibited in Fig. 6. TaON, TaON/CdS and TaON/CdS/ZnS films all displayed a luminescence band centered at 710 nm. The photoluminescence efficiencies of TaON/CdS and TaON/CdS/ZnS photocatalysts were both greater than the pure TaON film, especially the TaON/CdS/ZnS photocatalyst film. This may have resulted from the significant reduction in the density of the nonradiative transition recombination sites for photocatalytic composite films, particularly in TaON/CdS/ZnS. Furthermore, pure TaON could serve as effective capture traps for photogenerated carriers due to the reduced Ta species possessing a lower conduction band position than TaON. The low photoluminescence intensity of pure TaON was considered to reflect an increase in the prevalence of nonradiative transitions in the photocatalytic film. The identical trend in the photoluminescence and photocatalytic activity was reported in the TaON and TaON–ZrO2 photocatalysts. As a result, the pure TaON photocatalyst with low photoluminescence intensity exhibited reduced photocatalytic performance as compared to the composite photocatalyst films.62
To further verify the separation rates of the photogenerated electron and hole pairs, the transient photocurrents of the TaON, TaON/CdS and TaON/CdS/ZnS photocatalytic films were conducted under visible light irradiation. As displayed in Fig. 7a, all the films exhibited a quick response to the incident light on–off circulation: in particular, the TaON/CdS/ZnS composite photocatalysts showed greater enhancement in the transient photocurrent as compared to the pure TaON and TaON/CdS films. The improved photocurrent of the TaON/CdS/ZnS photocatalysts distinctly revealed the efficient photo-induced charge separation efficiency. Some spike peaks appeared in the I–t plots of the pure TaON and TaON/CdS photocatalytic films, which were attributed to the slower surface water oxidation reaction kinetics and faster recombination of photogenerated carriers for the TaON and TaON/CdS films. However, benefiting from the ZnS passivation, TaON/CdS/ZnS films presented remarkable photocurrent density along with a very stable photocurrent trend. Therefore, with the CdS nanoparticle deposition and ZnS passivation on TaON films, the TaON/CdS/ZnS films demonstrated the high efficiency of the photogenerated charge separation and transfer, thus leading to excellent photocatalytic capacities. Electrochemical Impedance Spectroscopy (EIS) was carried out to obtain deep insight into the photo-generated carrier transfer and separation performance and the synergistic effect of surface water oxidation kinetics for all photocatalyst films. Fig. 7b shows that TaON/CdS/ZnS films exhibited the smallest arc radius among the plots for all the films, consistent with the transient photocurrent measurements. Table 1 shows that the Rs values, as well as the Rct values of the TaON/CdS/ZnS film, were the smallest among all the photocatalytic films. These results fully illustrated that the TaON/CdS/ZnS photocatalytic films possessed the lowest resistance, thus promoting the efficient separation and transfer of photo-induced charge carriers and resulting in the enormous enhancement of the NO2 photodegradation efficiency.
Fig. 7 (a) Transient current plots (I–t) and (b) Nyquist plots of TaON, TaON/CdS and TaON/CdS/ZnS films under the irradiation of visible light. |
Photocatalytic film | Rs (Ω) | Rct (Ω) |
---|---|---|
TaON | 71.5 | 21970 |
TaON/CdS | 61.7 | 17650 |
TaON/CdS/ZnS | 52.5 | 9706 |
It was found that the TaON/CdS/ZnS photocatalytic films displayed a higher photocurrent as compared to the pure TaON and TaON/CdS films, which represented the more efficient water oxidation reaction kinetics. The excellent photoelectrocatalytic activity was generally due to the restrained recombination of photo-generated electron and hole pairs. The recombination occurred not only on the surface but also in the bulk of all the films. It is well known that benefiting from the lower reduction potential and faster water oxidation kinetics, H2O2 could be easily oxidized to remove the photo-induced holes.63 Therefore, H2O2 served as the sacrificial reagent of holes in the LSV measurements to demonstrate the photogenerated carrier transfer process. As exhibited in Fig. 8, pure TaON, TaON/CdS and TaON/CdS/ZnS films all showed improved photocurrents with the addition of H2O2 to the Na2SO4 electrolyte. The pure TaON films presented a greater increase than TaON/CdS and TaON/CdS/ZnS films in the presence of H2O2, which distinctly disclosed that H2O2 greatly facilitated the injection of holes into the electrolyte and lightened the surface recombination of pure TaON films. However, TaON/CdS and TaON/CdS/ZnS films displayed relatively small improvements, especially the TaON/CdS/ZnS photocatalyst. This indicated that the TaON/CdS/ZnS composite films possessed the least surface recombination due to the simultaneous deposition of CdS and ZnS onto TaON films, thus leading to the remarkable photoelectrocatalytic performance.
Fig. 8 LSV plots of (a) pure TaON film, (b) TaON/CdS film and (c) TaON/CdS/ZnS film tested in 0.5 M Na2SO4 electrolyte in the presence or absence of H2O2 with the irradiation of visible light. |
NO2 photocatalytic degradation experiments for all fabricated films aimed to further study the photocatalytic performance for the TaON film with the synergistic effects of CdS deposition and ZnS passivation. The NO2 photodegradation measurements were carried out under visible light irradiation and the effective area was 1 cm2 for all photocatalytic films. As exhibited in Fig. 9a, the concentration of NO2 showed a slight decrease without any photocatalyst after 2 h of visible light irradiation, which may be due to the equilibrium conversion between NO2 and other gases. Pure TaON film presented higher NO2 degradation efficiency reaching about 72.6% after only 2 h of light illumination. However, the NO2 photodegradation rate of the TaON/CdS film was barely improved, indicating the deposition of CdS nanoparticles on the TaON film. From this unusual phenomenon, it can be inferred that the slight enhancement of NO2 degradation for the TaON/CdS film may be due to the intense photo corrosion of CdS itself and the strong oxidizing property of NO2. Nevertheless, benefiting from the ZnS passivation layer at the outermost layer of TaON/CdS, the TaON/CdS/ZnS film exhibited remarkably increased NO2 degradation efficiency as compared to the pure TaON film, which achieved 96.7%. Therefore, this result leads us to conclude that ZnS passivation could greatly prevent the photo corrosion of CdS, thus resulting in the very beneficial photocatalytic performance of the TaON/CdS/ZnS film. The repeated NO2 photodegradation experiment was performed to further determine the recyclability and stability of the TaON/CdS/ZnS photocatalytic film. There was less than 6% reduction of the NO2 degradation efficiency after four degradation cycles, as shown in Fig. 9b. The XRD patterns of the cycled NO2 photodegradation over the TaON/CdS/ZnS film are also exhibited in Fig. S6.† These results demonstrated that ZnS as the passivation layer caused the composite film to exhibit outstanding photocatalytic performance and also excellent durability for NO2 photodegradation under visible light irradiation.
The trapping tests were also conducted to further investigate the active species that played a major role in the degradation of NO2. In the scavenger experiments, K2Cr2O7, KI, isopropyl alcohol (IPA) and p-benzoquinone (PBQ) served as the trapping reagents for the electrons (e−), photo-induced holes (h+), hydroxide radicals (˙OH) and superoxide radicals (˙O2−).64 From Fig. 10, it was observed that the NO2 degradation rates all exhibited varying degrees of decrease. We found that the degradation efficiency displayed an inconspicuous decrease with the addition of IPA, which manifested that ˙OH was not the dominant active species. The addition of K2Cr2O7 resulted in a slight decline in the NO2 removal rate, indicating that e− was an active species. However, after the addition of KI, the fairly obvious decrease of the NO2 degradation rate was noticed, which proved that h+ greatly contributed to the NO2 photocatalytic degradation. Furthermore, the rate presented the most significant reduction in the presence of PBQ, which demonstrated that ˙O2− played the most significant role in the NO2 photodegradation over the TaON/CdS/ZnS film under the illumination of visible light.
From the discussion above, we can conclude that the TaON/CdS/ZnS film exhibited superior photocatalytic activity for NO2 elimination under visible light irradiation. The possible charge carrier transfer mechanisms for the significantly improved photocatalytic performance of the TaON/CdS/ZnS photocatalytic film are illustrated in detail in Fig. 11. The trapping tests suggested that ˙O2− played the most significant role in NO2 photodegradation over the TaON/CdS/ZnS film. The conduction band (CB) position of TaON (−0.3 V) is more positive than the O2/˙O2− (−0.33 V vs. NHE) position, thus the electrons in the CB of TaON cannot reduce O2 to ˙O2−.55,65 Therefore, a direct Z-scheme transfer mechanism could be constructed to explain the enhanced photocatalytic activity for NO2 elimination.66,67 At first, CdS and TaON were excited to produce photoinduced carriers under the irradiation of visible light, and the electrons in the CB of TaON recombined immediately with the photoinduced holes on the VB of CdS, which greatly promoted the effective separation of photogenerated electron–hole pairs. Then, due to the more negative CB position (−0.9 V), the electrons in the CB of CdS were captured by O2 to promote the formation of active species ˙O2− on the photocatalytic film surface, and NO2 molecules reacted with ˙O2−, producing the final degradation products. At the same time, the remaining photogenerated holes in the valence band (VB) of TaON will also be used to remove NO2. There are some zinc vacancies (VZn) and interstitial sulfur vacancies (Is) in the ZnS passivation layer that serve as hole acceptors produced in CdS.68 Therefore, the holes in the VB of CdS partly migrate directly to (VZn) and (Is) in ZnS, which greatly facilitates the effective charge separation and ZnS displays excellent resistance to the reduced photo-corrosion of CdS. Therefore, the proposed mechanism above is probably responsible for the extraordinary photocatalytic degradation of NO2 for TaON/CdS/ZnS film.
Fig. 11 A possible schematic diagram for NO2 photodegradation over the TaON/CdS/ZnS film under the irradiation of visible light. |
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0ra01056a |
‡ These authors contributed equally to this work. |