Guanfeng Lin*abc,
Qiong Wangc,
Xuan Yangc,
Zhenghan Caic,
Yongzhi Xiongc and
Biao Huangc
aJinshan College, Fujian Agriculture and Forestry University, Fuzhou 350002, China. E-mail: feton.lin@hotmail.com
bKey Laboratory of Bio-based Material Science & Technology (Northeast Forestry University), Haerbin 150040, China
cMaterials Engineering College, Fujian Agriculture and Forestry University, Fuzhou 350002, China
First published on 6th May 2020
Biomass-derived porous carbon has received increasing attention as an energy storage device due to its cost-effectiveness, ease of manufacture, environmental friendliness, and sustainability. In this work, phosphorus-doped porous carbon was prepared from biomass sawdust (carbon source) and a small amount of phosphoric acid (P-doping source and gas expanding agent) by one-step carbonization. For comparison, parallel studies without phosphate treatment were performed under the same conditions. Benefiting from the addition of phosphoric acid, the prepared carbon material has higher carbon yield, higher specific area and micropore volume. Due to the heteroatom doping of P in the carbon material, the optimized PC-900 sample not only exhibits high specific capacitances of 292 F g−1 and 169.4 F g−1 at current densities of 0.1 A g−1 and 0.5 A g−1, respectively, but also excellent cycle longevity (98.3% capacitance retention after 5000 cycles) in 1 M H2SO4. In addition, the supercapacitor exhibits a high energy density of 10.6 W h kg−1 when the power density is 224.8 W kg−1 at a discharge current density of 0.5 A g−1. This work proposes a sustainable strategy to reuse waste biomass in high-performance and green supercapacitors for advanced energy storage equipment.
As reported in the literature, pure carbon materials can provide only limited catalytically active sites, and heteroatom doping is thought to cause redistribution of charges between carbon atoms, thereby activating small molecules.19 Therefore, heteroatom doping (e.g., O, N, P, S, B) is elected as a useful method to enhance the capacitive performance of carbon materials.9,20–24 Among them, the main reasons for choosing P are lower electronegativity and larger covalent radius. The lower electronegativity (2.19) of P atom compared to that of C atom (2.55) and the high electron donating property of the P atom makes the P dopant positively charged, which is advantageous for charge transfer.20 In addition, a much larger covalent radius of P (107 ± 3 pm) than C (73 ± 1 pm) causes many defects in the carbon material skeleton.19 These defects concentrate a large amount of charge, which may be the main active site. Therefore, with these unique characteristics of the P atom, P could be an ideal dopant for carbon.
At present, there have been reports of phosphorus-doped carbon as electrodes.25–27 However, there are only a few reports on the preparation of phosphorus-doped porous carbon electrodes using biomass as a raw material. A phosphorus-doped porous carbon, prepared using leaves as raw materials and phosphoric acid as a phosphorus dopant and its application in sodium ion and lithium ion batteries was reported by Zhu et al.28 Jiang et al. used NaH2PO4 as a P-doping source to prepare P-doped carbon derived from pinecone as an efficient catalyst for a Li–O2 battery.19 Nirosha et al. reported on preparation of phosphorus-doped carbon for asymmetric supercapacitors using Elaeocarpus tectorius as a carbon source and phosphoric acid as phosphorus.29 It is worth noting that the weight ratio of the raw material to the phosphorus dopant in the above work is relatively high, ranging from 1:2 to 1:10. In this work, in order to reduce the amount of phosphorus dopant and then reduce production cost, a small amount of phosphoric acid (the mass ratio of sawdust to phosphoric acid is 1:0.03) was used as a phosphorus dopant to prepare a phosphorus-doped porous carbon by one-step carbonization.
Based on these ideas, we developed a simple method for preparing P-doped porous carbon for electrode materials of supercapacitors, using sawdust and a small amount of phosphoric acid as raw materials. Sawdust is the main source of carbon. Phosphoric acid acts as a P-doping source and a gas expanding agent. To achieve high capacitance by doping phosphorus atoms into a carbon matrix, sawdust was carbonized with and without phosphoric acid at different temperatures of 700, 800, 900 and 1000 °C. A series of characterization methods were used to evaluate P-doped AC to clarify the role of phosphoric acid at different temperatures. In conclusion, this work is expected to provide new insights for the use of extremely simple methods to make heteroatom-doped materials as electrode materials for supercapacitors.
The electrochemical properties of the electrodes were evaluated in a three-electrode system, via VMP3 instrument (Bio-Logic, France) at room temperature. A 1 M H2SO4 aqueous solution was used as the electrolyte. In the three-electrode system, porous carbon electrode, Pt foil and Hg/HgO were used as working, counter, and reference electrodes, respectively. In the two-electrode system, both the positive and negative were the above-mentioned working electrode. Cyclic voltammetry (CV) experiments were performed at a potential range of 0–0.8 V, with a scan rate of 5 to 100 mV s−1. For galvanostatic charge/discharge (GCD) measurement, the current density varied within the range of 0.1–10 A g−1. The frequency of electrochemical impedance spectroscopy (EIS) analysis was 0.1 Hz to 106 Hz.
The specific capacitance (C, F g−1) of the electrode was calculated from the GCD curve, according to the following equation:11
C = IΔt/mΔV | (1) |
E = C × ΔV2/(2 × 3.6) | (2) |
P = E × 3600/Δt | (3) |
The N2 adsorption–desorption isotherms and pore size distribution (PSD) of samples with and without H3PO4 treatment at different carbonization temperature are presented in Fig. 3. And the pore structure parameters of the samples are presented in Table 1. For PC-X, all samples showed a typical type I, and the N2 adsorption–desorption isotherms showed a sharp increase in adsorption at P/Po < 0.05, which reflects the advantages of micropores. For C-X, the shape of the isotherm was an I/IV type curve, and it had an obvious hysteresis loop in the high-pressure range, which could be attributed to the micropore and mesopore characteristics. At high temperatures, H3PO4 can act as a catalyst to promote bond cleavage reactions and the formation of crosslinks. Therefore, it might develop the micropores during pyrolysis. As shown in Table 1, as the carbonization temperature increases, the specific surface area (SBET) and total pore volume (Vtot) of C-X and PC-X first increased and then decreased, and the SBET and Vtot of C-900 and PC-900 reached as high as 1094.0 m2 g−1, 0.829 cm3 g−1 and 1281.6 m2 g−1, 0.638 cm3 g−1, respectively. PC-X samples with H3PO4 exhibited a greater SBET and Vtot than that of C-X samples without H3PO4 at temperatures of 800 °C and 900 °C, indicating that a small amount of H3PO4 is an effective activated agent (gas expanding agent) at this temperature. However, when the temperature was 700 °C and 1000 °C, the SBET and Vtot of samples with H3PO4 were smaller than C-X samples without H3PO4. This is due to the fact that at temperatures above 750 °C, the gas produced by partial decomposition of H3PO4, (4H3PO4 + 10C → P4 + 10CO + 6H2O) will lead to the development of pore structure.29 Therefore, when the temperature is lower than 750 °C, H3PO4 will not decompose, so it cannot promote the enhancement of pore structures. When the temperature is too high (1000 °C), the decomposed gas quickly escapes, destroying the preliminary structure of the activated carbon. Suárez-García et al. reported that the volatilization of P-compounds promoted a new increase in wider micropores and narrow micropores.33 It was observed that the micropore surface area (Smic) and micropore volume (Vmic) of PC-X at the same temperature was higher than that of C-X, and the average pore size (d) showed the opposite trend, which further demonstrates that H3PO4 can develop micropores during pyrolysis. The pore size distributions of C-X and PC-X are shown in Fig. 3. The pores for C-X and PC-X were composed mainly of micropores (<2 nm), especially subnanopores (<1 nm). The main subnanopores of 0.5 to 1 nm provide accessible locations for penetration of aqueous electrolyte ions, thereby enhancing capacitance. C-X and PC-X also contained a small part of mesopores, which could be used as ion transport pathways. In addition, the mesopores of C-X were higher than that of PC-X. These results indicate that the presence of a small amount of H3PO4 is beneficial to the preparation of activated carbon with a microporous concentration.
Samples | SBET (m2 g−1) | Smic (m2 g−1) | Vtot (cm3 g−1) | Vmic (cm3 g−1) | D (nm) |
---|---|---|---|---|---|
C-700 | 804.2 | 442.2 | 0.483 | 0.207 | 2.40 |
PC-700 | 743.0 | 603.6 | 0.382 | 0.286 | 2.06 |
C-800 | 844.7 | 548.4 | 0.490 | 0.259 | 2.32 |
PC-800 | 1059.2 | 706.1 | 0.540 | 0.330 | 2.04 |
C-900 | 1094.0 | 468.5 | 0.829 | 0.453 | 3.03 |
PC-900 | 1281.6 | 835.6 | 0.638 | 0.535 | 1.99 |
C-1000 | 976.6 | 412.6 | 0.713 | 0.191 | 2.92 |
PC-1000 | 875.9 | 725.0 | 0.438 | 0.343 | 2.00 |
XRD patterns of C-X and PC-X are shown in Fig. 4. Two broad peaks centered at 24° and 43° can correspond to the (002) and (100) crystal planes, indicating the amorphous graphitic structure of the sample.34 The (002) plane of C-X and PC-X showed a shift from 26.4° of graphite to a lower value of 23.4–24.7°, which indicates an expansion in interlayer spacing. For C-X samples without H3PO4, as the carbonization temperature increased, its peak values (002) gradually approached 26.4°, which indicates that the increase in temperature promoted the generation of porous carbon graphitized crystallites. For PC-X samples with H3PO4, the peak values (002) of PC-700, PC-800, and PC-900 were almost the same, while the peak value of PC-1000 was far from 26.4°. This could be due to the flat deformation of graphite caused by the addition of a small amount of H3PO4. Interestingly, Compared to C-X, PC-X had a reduction in peak values (002) at 800, 900 and 1000 °C, especially at 1000 °C. This is because during the high-temperature heat treatment, the gas generated by the decomposition of phosphoric acid increases the interlayer spacing (consistent with the results of SEM analysis) and reduces the degree of graphitization of porous carbon.
Moreover, the higher the temperature, the faster the gas volatilizes, and the greater the interval between the carbon matrix layers. Panja et al. reported that P is likely to be incorporated into the edges of the graphene, which might widen the interlayer spacing.35 To further verify the graphitization of porous carbon with and without phosphoric acid, C-900 and PC-900 were selected for Raman spectra analysis. Fig. 4b shows the Raman spectra of C-900 and PC-900. The two discrete broad peaks around 1320 and 1580 cm−1 are designated as D-band and G-band, respectively, and are related to disordered carbon and sp2-bonded carbons.36 As shown in Fig. 4b, IG/ID of C-900 was higher than that of PC-900, which implies that the degree of graphitization of P-900 is higher (consistent with the results of XRD analysis), and the addition of a small amount of H3PO4 could not only open closed pores, but also etch graphitized carbon to create a more disordered structure. In addition, the incorporation of heteroatoms in carbon atoms can cause edge defects on the carbon surface, leading to increased D-band intensity.29 Therefore, the PC-900 sample showed higher D-band intensity, indicating that the P-doping produced disorder.
The surface chemical composition of C-X and PC-X was further analyzed by XPS (Fig. 5 and S1†). As shown in Fig. 5 and S1,† the survey spectrum of C-X was composed mainly of C and O elements. The peak with binding energy of 284.7 and 533.3 eV represented C1s and O1s. Compared with C-X, PC-X had a tiny peak near 133.4 eV, which corresponds to P2p, indicating that adding a small amount of phosphoric acid can achieve the phosphorus doping of porous carbon. C-900 and PC-900 were performed by deconvolution analysis, and the deconvolution spectrum of C1s was divided into three main peaks, including 284.6 eV (CC), and 285.1 eV (C–C/C–P), and at 288.2 eV (CO).7,8 There were two peaks in the O1s spectrum (Fig. 5c), and the sample surface included 531.9 eV (CO/C–O–P) and 533.4 eV (C–O).11 P 2p can be divided into the tetrahedral C–PO3 (134.1 eV) and C3–PO (132.7 eV).3 It has been reported that the incorporation of heteroatoms such as N and P will provide electrochemically active sites, enhance the wettability of the electrolyte on the electrode surface, and thus improve electrochemical performance.29
Fig. 5 XPS spectra of C-900 and PC-900: (a) full spectrum, (b–d) deconvolution spectrum of C 1s, O 1s, and P 2p of PC-900. |
FE-SEM images of C-900 and PC-900 are shown in Fig. 6. The images showed the ordered porous network structure for C-900 and PC-900. Both samples had uniform pores that help promote ion migration and provide more accessible active sites in the carbon matrix. As shown in Fig. 6, PC-900 was relatively loosely arranged with many micropores in the carbon matrix. This is due to the fact that doping of phosphorus has a great influence on the morphology of the carbon matrix, which leads to the expansion of interlayer space and induces the development of pore structures. Therefore, the carbon surface provides an ionic buffer to enrich the electrolyte transport during the electrochemical process.
As shown in Fig. 7c, all GCD curves at 0.5 A g−1 were closed linear and presented an isosceles triangular shape, which is a typical indicator of capacitive behaviour. The discharge curve of PC-900 does not have a noticeable voltage drop, showing a small internal resistance and excellent conductivity. According to the GCD curve calculation, PC-900 showed the best performances, and the specific capacitance of the electrode material calculated at a current density of 0.5 A g−1 was 169 F g−1. Fig. 7d and S3† show the GCD curves of C-X and PC-X at different current densities. All GCD curves of C-X and PC-X electrodes were shown as linear and isosceles triangular shapes,40 indicating good electrochemical reversibility during charging/discharging storage. The calculated gravimetric (Cg) capacitances based on the GCD results are presented in Fig. 7e. As shown in Fig. 7e, the Cg capacitance of all samples decreased with increasing current density. This might be because ions cannot diffuse into all micropores to form an electric double layer, and some faradaic reactions caused by heteroatom functional groups might not occur at high current density. At the same time, at low current density, such as PC-900, the Cg capacitance was greatly reduced.
When the current density was increased from 0.1 A g−1 to 0.5 A g−1, the Cg capacitance was reduced by 41.99%. This is due to the side reactions and irreversible redox reactions that occur at low current densities, which reduce the Cg capacitance. PC-900 provided the highest Cg capacitance of 292, 169.4, 152.8, 136.5, 118.5 and 98.5 F g−1 at current densities of 0.1, 0.5, 1.0, 2.0 5.0 and 10.0 A g−1, respectively. Table 2 presents the electrochemical performance of various biomass-derived carbons prepared by different methods. Compared to other biomass-derived carbons, we can use a small number of chemical reagents to prepare porous activated carbon with good performance, and the method is low-cost and effective.
Biomass precursor | Preparation method | Mass ratio (biomass:reagent) | SBET | Cg capacitance | Measurement condition | Ref. |
---|---|---|---|---|---|---|
Eucommia ulmoides wood | Hydrothermal + H3PO4 | 1:3.3 | 1456 | 185 F g−1 | 1M H2SO4, 5mV s−1 | 41 |
Rubberwood | KOH | 1:2 | 1932 | 100 | 1.0 m Li-TFSI, 0.1 A g−1 | 42 |
Rubberwood | H3PO4 | 1:1 | 693 | 129 | 1 M H2SO4, 1mV s−1 | 43 |
Firewood | KOH | 1:1 | 1064 | 180 | 0.5 M H2SO4, 10 mV s−1 | 44 |
Pinecone | KOH | 1:1 | 1515 | 137 | 1 M Na2SO4, 0.1 A g−1 | 45 |
Elaeocarpus tectorius | H3PO4 | 1:3.4 | 858 | 201 | 1 M H2SO4, 1 A g−1 | 29 |
Borassus flabellifer flower | H3PO4 | 1:4.25 | 633 | 238 | 1 M KOH, 1 A g−1 | 46 |
Lignocellulose powders | NaH2PO4 + ZnCl2 | 1:(0.67 + 1.33) | 658 | 193.6 | 6 M KOH | 47 |
Fir sawdust | H3PO4 | 1:0.03 | 1281.6 | 292 and 169.4 F g−1 | 1 M H2SO4, 0.1 and 0.5 A g−1 | This work |
Compared with C-X, PC-X had a higher Cg capacitance at the corresponding temperature, which indicates that the electrochemical performance of porous carbon is enhanced after phosphorus doping. The doping of the P-functional group can improve the wettability of the electrode and directly generate a pseudocapacitance through a redox reaction. This reaction is presented later.29,48
To further understand the capacitive behavior, an electrochemical impedance spectroscopy (EIS) was tested. The Nyquist spectra of C-X and PC-X are shown in Fig. 7f. As shown in Fig. 7f, the EIS curves of C-X and PC-X were similar, consisting of a semicircle at high frequencies and a linear component at low frequencies. The line represented Warburg diffusion resistance, which comes from the ion diffusion of the electrolyte. It is generally accepted that the more perpendicular the straight line, the better the capacitive performance of porous carbon.3 Thus, at the corresponding temperature, the perpendicularity of PC-X is higher than that of C-X, which indicates that PC-X has better capacitance performance. A semicircle indicates the charge transfer resistance from electrode/electrolyte interface, whereas a smaller circle signifies a faster charge transfer rate.49 The presence of small semicircles reveals the pseudocapacitive behavior of porous carbon. Nian et al. pointed out that the semicircle of pseudocapacity was due to the interfacial redox reactions of impurities and surface functional groups.50 As shown in Fig. 7f, the semicircle of PC-X was smaller than that of C-X, which further indicates that the capacitance performance of PC-X is better. Compared with other electrodes, the vertical line of the PC-900 electrode was the largest, and the semicircle was the smallest, indicating that its diffusion and transfer resistance are lower.
Cycle stability is the most important feature determining whether or not a material can be put to practical use.51 The long-term cycle stability of PC-900 was evaluated under the high current density of 2 A g−1. After 5000 charge–discharge cycles, it showed excellent cycle stability with a capacitance retention rate of 98.3% (Fig. 8a). The inset of Fig. 8a shows the first and last cycles of the GCD curve, and they still show a symmetrical triangle shape during the cycle test, which indicates excellent electrochemical cycle stability.
Fig. 8 (a) specific capacitances and capacitance retention of PC-900 at 2A g−1 (the inset are the first cycle and the 5000th cycle of GCD of PC-900 at 2A g−1), (b) Ragone plots of PC-900. |
Energy density and power density are two practical parameters for evaluating supercapacitors, and they were calculated based on the GCD of a two-electrode system (Fig. S4†). The energy density and power density of PC-900 were calculated and summarized in the Ragone plot (Fig. 8b). As shown in Fig. 8b, the PC-900 based supercapacitor showed a high energy density of 10.6 W h kg−1 when the power density was 224.8 W kg−1 at the discharging current density of 0.5 A g−1. The obtained results show that the potential applications of PC-900-based supercapacitors in energy storage equipment are broad.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0ra02398a |