Yajie
Hu‡
,
Yanan
Yang‡
,
Jiejing
Zhang
,
Shengnan
Jin
and
Hong
Zheng
*
Beijing Key Laboratory of Materials Utilization of Nonmetallic Minerals and Solid Wastes, National Laboratory of Mineral Materials, School of Materials Science and Technology, China University of Geosciences, Beijing 100083, China. E-mail: zhengh@cugb.edu.cn
First published on 21st July 2020
The removal of low concentration PPCPs from water is a challenging issue. A graphene hydrogel with 3D networks shows great potential for accelerating eddy diffusion of low concentration PPCPs. Herein, to further promote its molecular diffusion, a graphene/TiO2 nanowires (GNW) hybrid structure was implanted into graphene hydrogel. The as-prepared rGO/GNW hydrogel exhibited significantly enhanced adsorption–photocatalytic performance and excellent stability for low concentration ethenzamide, a typical pharmaceutical pollutant in water, under vacuum ultraviolet (VUV), ultraviolet (UV), visible and near-infrared light irradiation. When the initial ethenzamide concentration was 500 ppb and catalyst dosage was 10 mg/150 mL, ethenzamide was completely removed in 3 min and the corresponding photocatalytic apparent rate constant was 2.20 times that by GNW, 4.09 times that by rGO/P25 and 4.31 times that by rGO/NW under VUV irradiation, respectively, and its removal rate attained 99.0% in 120 min and the corresponding photocatalytic apparent rate constant was 2.06 times that by GNW, 3.34 times that by rGO/P25 and 17.42 times that by rGO/NW under UV irradiation, respectively. The GNW hybrid structure in the hydrogel played a vital role in overcoming the mass transfer resistance of low concentration PPCPs. The as-prepared rGO/GNW hydrogel exhibits significant potential for the removal of low concentration PPCPs from water.
Generally, various wastewater treatment technologies such as advanced oxidation technology,10 activated carbon process,11 biological treatment technology,12 UV treatment technology13 and membrane separation technology14 are studied to remove PPCPs in water. However, for low concentration PPCPs, they are difficult to be efficiently removed by these conventional treatment technologies since their mass transfer resistance is difficult to be overcome. Photocatalysis is considered as a promising and ideal advanced treatment technology owing to its mild reaction conditions, strong mineralization ability to persistent pollutants without any chemical input or output and no sludge residue.15–21 While as a versatile semiconductor, TiO2 photocatalyst has been widely concerned due to its superior photocatalytic activity, excellent photochemical stability, low cost and low toxicity.22–24 Some efforts also have been tried to overcome the mass transfer resistance of low concentration PPCPs by doping TiO2 on microporous zeolite,25 preparing rice-shaped nanoporous TiO2 (ref. 26) and nanoporous TiO2 film with exposed {001} facets27,28 or implanting Pt single atoms on nanoporous TiO2 film.29 However, although abundant nanopores can considerably accelerate the eddy diffusion of low concentration PPCPs and atomically implanted noble metal can significantly accelerate molecular diffusion of low concentration PPCPs, either poor molecular diffusion or high cost of noble metal still limited their practical application.
In recent years, the practical use of rGO-based photocatalysts has attracted great attention.30–33 Graphene hydrogel with 3D graphene networks shows great potential for accelerating eddy diffusion of low concentration PPCPs due to its convenient mass transfer channels and rich pore structure.34,35 Moreover, easy recovery from aqueous solution is advantageous to its practical application.36 So, the rational construction of TiO2/graphene hydrogels can not only contribute to providing large specific surface area and high porosity, but also promoting the capture of light by active sites due to light refraction–reflection coming from 3D network structure.37 Furthermore, photogenerated electron–hole pairs of TiO2 can be efficiently separated owing to excellent electrical conductivity of graphene. Thereby, it is hopeful that both eddy diffusion and molecular diffusion coming from low concentration PPCPs are effectively overcome. In previous study, TiO2 nanoparticles were chemically bonded to graphene and formed TiO2 (P25)–graphene hydrogels, which exhibited a significant enhancement in the removal of methylene blue, in comparison with sole P25.38 However, lower specific surface area and more agglomeration greatly limited eddy diffusion and molecular diffusion coming from low concentration PPCPs.
Herein, to overcome the agglomeration of TiO2 in hydrogel and form stable TiO2/graphene hydrogel with larger specific surface area and higher active sites to effectively promote eddy diffusion and molecular diffusion of low concentration PPCPs, graphene/TiO2 nanowire (GNW) hybrid structure was prepared first and then used to bond to graphene and form reduced graphene/GNW (rGO/GNW) hydrogel. The as-prepared hydrogel exhibited highly efficient adsorption–photocatalytic activity and excellent stability for the removal of low concentration ethenzamide, a typical pharmaceutical pollutant in water, under VUV, UV, visible and near-infrared light irradiation. The GNW hybrid structure in the hydrogel contributed to uniform dispersion of TiO2 nanowires on graphene and chemical bonding between graphene and TiO2 nanowires, and played a vital role in promoting eddy diffusion and molecular diffusion of low concentration PPCPs.
The samples were characterized by TEM, FESEM, XRD, Raman, UV-Vis DRS, XPS, BET, FTIR, PL, EIS determination. Detailed test conditions and instrument model can be found in ESI.†
To examine the stability of the as-prepared rGO/GNW, the adsorption and photocatalytic experiments of ethenzamide were repeated for three times under VUV and UV light irradiation, respectively. After each one, the as-prepared rGO/GNW was separated and directly used for next test.
XRD patterns and Raman spectra of the samples are shown in Fig. 2. From the XRD patterns (Fig. 2a), we can see that the diffraction peak of GO at 2θ = 10.5° disappeared in GNW, rGO, rGO/NW, rGO/GNW and a new wide diffraction peak of rGO appeared in rGO, rGO/NW and rGO/GNW, confirming that elimination of oxygenated functional groups and the existence of strong π–π stacking interactions between the rGO nanosheets contributing to gelation in these samples.39 No wide diffraction peak of rGO was observed in GNW, indicating no gelation occurred, which is consistent with the TEM results of GNW. Possible reason was attributed to low content of rGO in GNW. The diffraction peaks of TiO2 could be clearly observed in GNW and rGO/GNW, indicating that the crystal structure of TiO2 was not destroyed by the hybrid and gelation processes.
Raman spectra further provided structural details of the samples. As shown in Fig. 2b, all the samples containing TiO2 including NW, GNW, rGO/P25, rGO/NW and rGO/GNW revealed the TiO2 characteristic absorption bands at 149 cm−1 (E1g), 396 cm−1 (B1g), 516 cm−1 (A1g) and 639 cm−1 (Eg), confirming the existence of TiO2. While the D band corresponding to the structural defects or partially disordered graphitic domains and the G band representing tangential C–C stretching vibrations presented in the spectra of all the samples containing graphene.41 The intensity ratio of the two bands, ID/IG, can be used to characterize short-ranged sp2 carbon moieties and sp3-hybridized carbon atoms in rGO, thereby, to evaluate the extent of defects/disorder in graphitic structures.39,41 The higher the number of sp3 defects/disorder is, the higher the ID/IG values are, implying that the smaller the average size of the sp2 carbon moieties is and hence the higher the degree of GO reduction is. Compared with ID/IG ratio of GO (1.9), that of GNW (2.5) increased significantly, indicating that the average size of sp2 carbon moieties decreased significantly and reduction of GO was significantly increased by the hybrid process. Moreover, in comparison with the ID/IG ratios of rGO (2.3), rGO/P25 (3.1) and rGO/NW (3.8), that of rGO/GNW (4.0) also increased significantly, indicating there was a strong interaction between GNW and rGO nanosheets39 and GNW hybrid structure increased disorder of rGO flakes.
To investigate the effect of GNW hybrid structure on the specific surface area and pore size of the as-prepared hydrogel, adsorption–desorption curves and corresponding pore-size distribution of the samples were determined, the results are shown in Fig. 3. It can be observed that adsorption isotherms of rGO, rGO/P25 and rGO/GNW were of IV type isotherms (BDDT classification), suggesting the existence of mesopores (2–50 nm), which is consistent with the results of pore-size distribution in the inset of Fig. 3. Moreover, we can also see that the main pore size of rGO hydrogel was about 17 nm, while those of rGO/P25 and rGO/GNW were about 10 nm and more such pores existed in rGO/GNW, which is consistent with FESEM results. Compared with the specific surface area of rGO/P25 (68 m2 g−1), that of rGO/GNW (106 m2 g−1) obviously increased, further confirming that GNW hybrid structure is advantageous for overcoming the agglomeration of TiO2 nanowires although it was slightly lower than that of rGO hydrogel (132 m2 g−1) due to the inclusion of GNW.
Fig. 3 Adsorption–desorption curves and corresponding pore-size distribution (inset) of the samples. |
FTIR spectra were used to further examined the functional groups and chemical bond in the samples (Fig. 4). In comparison with GO, the absorption peak intensities of some oxygen-containing functional groups in GNW including epoxy or alkoxy C–O (1045 cm−1), epoxide C–O–C or phenolic C–O–H (1229 cm−1), CC (1626 cm−1), carboxylate or ketone CO (1735 cm−1) and water –OH (1626 cm−1 and 3415 cm−1)39,42,43 obviously weakened or disappeared, confirming the reduction of GO by hydrazine hydrate and ascorbic acid in the hybrid process. The broad absorption peaks around 400–1000 cm−1 in GNW corresponded to Ti–O–Ti and Ti–O–C vibration, confirming the formation of a chemical bond between the rGO and TiO2 nanowires,44 which is consistent with Raman results. The chemical bond contributed to the dispersion of TiO2 nanowires on the surface of graphene and the formation of stable rGO/GNW hydrogel. The absorption peak intensities of some oxygen-containing functional groups in rGO/GNW and rGO/P25 further weakened or disappeared, confirming that GO was further reduced by hydrazine hydrate and ascorbic acid in the gelation process. The peak at 1569 cm−1 in rGO/GNW could be ascribed to the sp2 hybridization of carbon with adjacent carbon atoms in the graphene sheet and formation of CC double bond, implying that GNW and rGO were tightly combined by the chemical bond.
To further investigate the surface elemental composition and chemical state of the samples, XPS spectra were determined and are shown in Fig. 5. The presence of Ti, O and C elements in the survey spectra of GNW and rGO/GNW (as shown in Fig. 5a) was consistent with their composition. By fitting the high-resolution spectra of C1s (Fig. 5b), it can be seen that the peaks centered at 284.7 eV, 285.1 eV, 286.6 eV and 288.6 eV corresponded to C1s of C–C, C–O, C–OH and CO in rGO hydrogel, respectively.45,46 In comparison with C1s of rGO, the presence of Ti–O–C bond in GNW and rGO/GNW further confirmed the formation of chemical bond between TiO2 nanowires and graphene nanosheets, which contributed to the dispersion of TiO2 nanowires on the surface of graphene and the formation of stable GNW hybrid structure and rGO/GNW composite. Moreover, the chemical bond could be used as the channel for the efficient transfer of photogenerated carrier.45 In the high-resolution XPS spectra of O1s (Fig. 5c), O1s in GNW could be divided into three peaks centered at 529.5 eV, 530.5 eV and 531.4 eV, which were assigned to Ti–O bond, oxygen vacancies (Ov) and adsorbed water,47 respectively. In comparison with GNW, the bonding energies corresponding to the lattice oxygen and Ov in rGO/GNW shifted towards higher binding energy, which was ascribed to the strong interaction between GNW hybrid structure and rGO nanosheets in the process of gelation. The high-resolution spectra of Ti2p (Fig. 5d) could be divided into four peaks corresponding to Ti4+ 2p1/2, Ti3+ 2p1/2, Ti4+ 2p3/2 and Ti3+ 2p3/2, respectively. Similarly, in comparison with GNW, the bonding energies corresponding to Ti4+ and Ti3+ in rGO/GNW also shifted towards higher binding energy, which was consistent with high-resolution spectra of O1s. On the basis of the high-resolution spectra of O1s and Ti2p, it can be seen that Ov and Ti3+ were successfully introduced into GNW and rGO/GNW due to the reduction by reducing agents in the process of hybrid and graphene gelation. Ti3+ and Ov could form a new sublevel state at the bottom of the conduction band (CB) of TiO2 and narrow the band gap of rGO/GNW,47 which was advantageous to the absorption of long wavelength light. The strong interaction between GNW hybrid structure and rGO nanosheets could accelerate the separation of photogenerated carriers.
To investigate the light absorption property of rGO/GNW, the UV-Vis DRS spectra of the samples were determined (Fig. 6). Compared with TiO2 nanowires, the light absorption performance of rGO/GNW was obviously improved. Similar to GNW, light response range of rGO/GNW was expanded to near-infrared region, indicating that the rGO/GNW has potential photocatalytic property in the whole spectrum region. However, in comparison with TiO2 nanowires, in spite of the absorption spectra of rGO/NW shifted slightly towards long wavelength, much weaker light absorption than rGO/GNW was found. Possible reason was ascribed to the formation of Ti–O–C at the interface between TiO2 nanowires and rGO in GNW hybrid structure.48,49
Fig. 7 Adsorption, photocatalytic degradation (a) and corresponding photocatalytic apparent rate constants (b) of ethenzamide under VUV irradiation by the different samples. |
Fig. 8 shows the experimental results under UV irradiation. Similarly, the equilibrium adsorption rate of ethenzamide by the as-prepared rGO/GNW under the experimental conditions (Fig. 8a) obviously improved and reached 30%, which was far higher than other samples. Different equilibrium adsorption rate from that under VUV irradiation was attributed to different experimental apparatus. After 120 min under UV irradiation, the removal rate of ethenzamide attained 99.0%, which was also much higher than those by other samples. The corresponding UV photocatalytic apparent rate constant during the first 30 min (Fig. 8b) was 2.06 times that by GNW, 1.91 times that by NW, 3.34 times that by rGO/P25, 17.42 times that by rGO/NW and 3.98 times that by P25. Low photocatalytic activity of rGO/NW was ascribed to the separation of TiO2 nanowires from graphene. The rate constant normalized to the specific surface area (Fig. S5b†) also indicated that GNW contributed to UV photocatalytic degradation of ethenzamide. These results further confirmed that both GNW hybrid and 3D network structure of hydrogel play an indispensable role in removing low concentration ethenzamide.
Fig. 8 Adsorption, photocatalytic degradation (a) and corresponding photocatalytic apparent rate constants (b) of ethenzamide under UV irradiation by the different samples. |
The experimental results under visible and near-infrared light irradiation are shown in Fig. 9. Similarly, the removal rate of ethenzamide by the as-prepared rGO/GNW attained 87.0% under visible light irradiation for 8 h and 86.2% under near infrared light irradiation for 12 h after adsorption equilibrium, respectively, which was also much higher than those by NW (10.6% and 10.0%, respectively) and GNW (29.9% and 29.1%, respectively). The corresponding visible photocatalytic apparent rate constant during the first 6 h was 4.38 times that by GNW, 17.50 times that by NW and near-infrared photocatalytic apparent rate constant during the first 8 h was 4.00 times that by GNW, 20.00 times that by NW, indicating that the as-prepared rGO/GNW has a good adsorption and full spectrum photocatalytic performance for the removal of low concentration ethenzamide.
Fig. 9 Adsorption and photocatalytic degradation of ethenzamide under visible (a) and near-infrared light (b) irradiation by the as-prepared rGO/GNW. |
To evaluate the stability and reusability of the as-prepared rGO/GNW, the adsorption and photocatalytic degradation of ethenzamide under VUV and UV light irradiation were repeated for three times. Almost no deactivation was found except for 6% decrease of removal rate of ethenzamide under UV light irradiation after 3 recycling uses (Fig. 10), indicating that the as-prepared rGO/GNW has excellent adsorption and photocatalysis stability and can serve as an efficient and stable adsorption and photocatalytic material with full spectrum response for the removal of low concentration ethenzamide.
Fig. 10 Cycling runs of the as-prepared rGO/GNW for adsorption and photocatalytic degradation of ethenzamide under VUV (a) and UV (b) light irradiation. |
To explicit the active species in the process of photocatalytic reaction, ammonium oxalate, N2 and tert-butyl alcohol (TBA) were used as the capture agents of holes (h+), superoxide radicals (˙O2−) and hydroxyl radical (˙OH), respectively and the results are shown in Fig. S7.† It can be seen that the photocatalytic activity of the as-prepared rGO/GNW was significantly inhibited by the addition of ammonium oxalate, N2 and TBA, especially for ammonium oxalate and TBA, the photocatalytic degradation of ethenzamide almost was completely inhibited. Thereby, it could be inferred that h+, ˙OH and ˙O2− played a vital role in the process of the photocatalytic reaction.
On the basis of the above experimental results, a possible adsorption–photocatalysis mechanism for the removal of low concentration ethenzamide by the as-prepared rGO/GNW was proposed, as shown in Fig. 11. Firstly, rGO/GNW hydrogel with 3D graphene networks can contribute to accelerating eddy diffusion of low concentration ethenzamide owing to its convenient mass transfer channels and rich pore structure, thereby, more ethenzamide was adsorbed to active sites of rGO/GNW. Then, TiO2−x with a narrower band gap in rGO/GNW than TiO2 can be easily excited by light to generate electrons and holes. At the same time, refraction–reflection coming from 3D network structure can promote the capture of light by active sites. Furthermore, photogenerated electrons of TiO2−x in rGO/GNW enter the conduction band of TiO2 and can smoothly transferred to graphene sheets owing to the higher potential of graphene/graphene˙− (−0.08 V vs. SHE) than the conduction band position of TiO2 (−0.24 V vs. SHE)48,52 and favorable channel coming from the chemical bond between NW and graphene nanosheets, as well as GNW and rGO.45 The separated electrons can be caught by oxygen molecule adsorbed on the as-prepared rGO/GNW to form ˙O2−. ˙O2− can further react with H+ in the aqueous solution to form H2O2 and generate ˙OH.45 Simultaneously, the holes located in VB can oxide OH− or adsorbed water molecules to generate ˙OH.47 As a result, the ethenzamide adsorbed on the surface of rGO/GNW is effectively degraded by these reactive oxidizing species including ˙O2−, ˙OH and h+. Moreover, oxygen vacancies can promote photocatalytic reaction as catalytic active center. Thereby, molecular diffusion of low concentration PPCPs is effectively promoted.
Fig. 11 Possible adsorption–photocatalysis mechanism of the as-prepared rGO/GNW for the removal of low concentration ethenzamide. |
The GNW hybrid structure in the hydrogel played a vital role in promoting uniform dispersion of TiO2 nanowires on graphene, chemical bonding between graphene and TiO2 nanowires, as well as GNW and graphene nanosheets, eddy diffusion and molecular diffusion of low concentration ethenzamide. The as-prepared rGO/GNW hydrogel exhibits significant potential for efficient adsorption and photocatalytic degradation of low concentration PPCPs in water.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0ra03449e |
‡ The first coauthors. |
This journal is © The Royal Society of Chemistry 2020 |