Lara Strohmeier,
Heike Frommwald and
Sandra Schlögl*
Polymer Competence Center Leoben, 8700 Leoben, Austria. E-mail: sandra.schloegl@pccl.at
First published on 22nd June 2020
This study highlights the additive manufacturing of diene-rubbers with digital light processing (DLP). The network formation relies on the crosslinking of a methacrylate-functional liquid isoprene rubber via photo-induced thiol-click chemistry. Bi-functional divinyl ethers are added as reactive diluents, which benefit from a low potential for skin irradiation and skin sensitization. Along with significantly reducing the viscosity, the divinyl ethers accelerate the cure kinetics of the diene-rubber across the main chain CC bonds of the isoprene units. Photo-DSC measurements reveal that the length of the glycol-spacer and the chemical structure (glycol versus alkyl) of the divinyl ether influence the photo-reactivity of the rubber formulations in thiol–ene reactions. In the present study, the highest reactivity is observed for tri(ethylene glycol) divinylether comprising a spacer with three glycol units. To improve the storage stability of the rubber formulation, a radical scavenger is applied to reduce premature crosslinking reactions under dark conditions. With the stabilized liquid rubber formulations, precise 3D structures with features of 0.5 mm are successfully manufactured with bottom-up DLP 3D printing.
For well-established AMTs based on UV curing processes (e.g. digital light processing, DLP, stereolithography, SLA and PolyJet), only a few photocurable elastomers are commercially available, including Carbon EPU 40,8 Stratasys TangoPlus,9 Formlabs Flexible,10 and Spot-A Elastic.11 Those elastomers are based on UV curable urethane acrylates and acrylates with flexible chains that provide the “soft domains” in the cured elastomer networks. By optimizing the composition of the urethane and acrylate monomers, researchers were able to fabricate 3D printed elastomer objects with an elongation of up to 1000%.12
Among the printing processes using light to build the object, DLP offers distinctive advantages since it provides high resolution and surface quality at low cost and comparably high throughput rates.13 It relies on a localized photopolymerization process which is initiated by light in the UV-vis region. The printing is carried out in a vat containing liquid monomers or oligomers and an appropriate photoinitiator.14 The resin formulation is selectively crosslinked layer-by-layer upon light exposure (Fig. 1b). In contrast to SLA, each layer is illuminated all at once using a selectively masked light source comprising binary patterns (information on each layer is provided in the form of black and white images) presented by a digital micro-mirror device. Thus, the build time is significantly shorter compared to SLA.
Whilst the DLP printing with urethanes has been successfully employed in the fabrication of stretchable objects, the DLP printing with diene-rubber materials is still in its infancy.15 Due to their salient features including high elasticity, strength, and recovery, diene-rubbers are applied in numerous technical applications.16 Along with classical sulfur and peroxide curing, several photochemical routes have been established to crosslink diene-rubbers over the past years.17,18
One of the most popular reaction mechanisms, is thiol–ene click chemistry, which enables the photo-induced crosslinking of diene-rubbers across their unsaturated carbon double bonds located either in the main or side chain.17,19,20 Further approaches involve the introduction of functional groups or chromophores into the rubber chains, which undergo crosslinking reactions upon UV exposure.21 In particular, acrylate or methacrylate groups are often exploited since they are well known for their high reactivity in radical induced chain growth reactions.22 Thus, diene-rubbers with functional acrylate groups undergo rapid crosslinking upon UV irradiation in the presence of an appropriate photoinitiator.23,24
For the DLP printing of diene-rubbers, liquid rubber formulations are required that provide a high photo-reactivity and a low viscosity to fabricate 3D objects with adequate resolution and printing speed. Recently, Scott and co-workers demonstrated the successful printing of a hydrogenated butadiene rubber.19 The photo-reactivity was obtained by functionalizing the liquid rubber with acrylate-groups. In addition, low-viscous acrylates were added as reactive diluents to increase the cure rate and to reduce the viscosity of the printing formulations.
In a similar approach, Nanni et al. used thiol-acrylate chemistry to print an acrylate-functionalized liquid butadiene rubber via a layer-by-layer deposition of liquid filaments with a syringe followed by a UV induced curing of each layer.20 However, due to the limitations of the printing technique, the printed objects were characterized by a rather poor resolution and surface quality.
Inspired by this work, we exploit the concept of thiol-click chemistry for the DLP 3D printing of liquid isoprene rubber. In particular, a commercially available liquid isoprene rubber with methacrylate side chains was used as base resin. Since acrylates and methacrylates are well known for their cytotoxicity and high irritancy potential, which limits their overall biocompatibility, we tried to keep the number of methacrylate functions in the formulation as low as possible.25 Thus, multi-functional divinyl ethers were used as reactive diluents, which undergo a photo-induced thiol–ene reaction across the carbon double bonds of the isoprene units (Fig. 1a). By optimizing type and concentration of the divinyl ether, DLP 3D printable resin formulations are obtained that are characterized by high curing rates and adequate printing quality.
For the pure methacrylate-functional liquid isoprene rubber used in the present study, a viscosity of 79 Pa s was determined at room temperature. To decrease the viscosity towards a processible level, selected divinyl ethers (Fig. 1a) were added to the liquid rubber. In addition, a multi-functional thiol and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide as well as ethyl(2,4,6-trimethylbenzoyl)phenylphosphinate were applied as long-wavelength absorbing photoinitators to cure the rubber formulation by photo-induced thiol–ene chemistry.
It should be noted that thiol–ene systems often suffer from premature polymerization due to a base-induced Michael addition of the thiol groups to the carbon double bonds of the “ene”. Furthermore, dark polymerization reactions can be initiated by hydroperoxide impurities or the generation of radicals through a ground-state charge.28
To determine the shelf-life of the rubber formulations, their viscosity was monitored under accelerated ageing conditions (50 °C for 24 h) (Fig. 2a). Independent on the type of reactive diluent, the viscosity of the rubber formulations significantly increased and with 101 Pa s LIR-SH-BD-ns even exceeded the initial viscosity of the pure liquid rubber.
To overcome the premature gelation of the rubber formulations, an emphasis was put on finding suitable stabilizer systems. Pyrogallol has been reported as one of the most efficient radical scavengers for thiol–ene systems due to its high resonance stabilization.29 However, the amount of pyrogallol has to be carefully chosen since the photo-reactivity will decrease upon the addition of radical stabilizers.30,31
Directly after mixing, the stabilized formulations comprised a viscosity between 1 and 6 Pa s, which is significantly lower than the viscosity of the non-stabilized ones (11–14 Pa s). The results clearly show that the non-stabilized samples start polymerizing immediately after preparation, which results in resin viscosities beyond the desired processing range. Although the viscosity of the stabilized formulations increased to 32–37 Pa s after prolonged storage at 50 °C, the shelf-life of the formulation at room temperature is sufficiently high for using them in the subsequent DLP 3D printing process.
In this context, it has to be considered that a sufficient storage stability for thiol–ene systems over weeks was only reported for synergistic stabilizer systems, which hinder both, the radical and basic induced dark reactions.30,31 However, optimizing the shelf-life of the rubber formulations was beyond the scope of this study.
Formulation | Peak height (mW mg−1) | Area (J g−1) | tmax (s) |
---|---|---|---|
LIR-REF | 0.6 | 10.8 | 7.6 |
LIR-SH-TEG | 8.7 | 82.3 | 7.7 |
LIR-SH-DEG | 5.3 | 58.1 | 7.6 |
LIR-SH-BD | 3.3 | 47.3 | 7.3 |
In the absence of any reactive diluent and thiol crosslinker, the methacrylate-functional isoprene rubber (LIR-REF) suffers from a low monomer conversion as revealed by the low height and small area of the released heat (Fig. 2). Even though tmax suggests a reasonably fast curing speed, the flattened and broad curve indicates a delay in monomer conversion.
The addition of the selected divinyl ethers together with the thiol crosslinker leads to a distinctive increase in both peak height and area of the heat enthalpy, which corresponds to higher monomer conversions. This is attributed to the higher number of functional groups and the lower viscosity of the rubber formulations upon the addition of the diluents. Reactive diluents lead to an increase in mobility and facilitate the diffusion of the monomers, which generates an overall higher monomer conversion.33 In contrast, tmax is not significantly changing, which suggests that tmax observed for the rubber formulations is mainly related to the reactivity of the photoinitiators.
For a more detailed information on cure kinetics and final monomer conversion, FTIR experiments were performed. FTIR spectra of the stabilized rubber formulation LIR-SH-TEG are shown in Fig. 3 prior to and after UV exposure.
To follow the curing process, the bands of the thiol groups (S–H stretching at 2572 cm−1), carbon double bonds of the divinyl ether (CC bending at 1641 cm−1) and the main chain carbon double bonds of the isoprene (CC–H wagging at 840 cm−1) were monitored. In order to calculate the monomer conversion, the area of the characteristic IR absorption bands were integrated and related to a reference band (CO stretching at 1720 cm−1). The normalized monomer signals were obtained by taking the ratio of the monomer bands to the reference band. Subsequently, the monomer conversion was calculated according to the following eqn (1) where t0 refers to the initial monomer band and t to the bands at the irradiation time t:
(1) |
For the reference (LIR-REF) system, the methacrylate groups (CC at 1641 cm−1) are consumed (conversion amounts to 20%) upon UV irradiation. In addition, a slight conversion of the main chain carbon double bonds (CC at 1666 cm−1) of the isoprene units was observed (Fig. S1 in ESI†). This is in accordance with the broadened peak observed in the photo-DSC experiments, which suggests that the radical induced short chain crosslinking of the isoprene double bonds takes place, albeit very slowly. The low conversion of the main chain CC bonds of the liquid rubber can be attributed to the low reactivity of non-activated (absence of electron withdrawing groups) carbon double bonds in radical induced addition reactions.24,34 In addition, previous work revealed that diene-rubbers with alkene groups in the side chain provide a higher reactivity in thiol–ene reactions than cis-1,4-poly(isoprene) rubber with CC groups in the main chain.35 However, photo-curing of cis-1,4-poly(isoprene) rubber either in solid film state or liquid latex state yielded similar crosslink characteristics than sulfur cured systems.36
In the present work, the crosslinking density of the liquid rubber could be significantly increased upon the addition of divinyl ethers as reactive diluents. FTIR data of the stabilized rubber resins reveal that the conversion of the main chain CC bonds of the isoprene units more than doubled (55–65%) for liquid rubber formulations containing thiol crosslinker and divinyl ether (Fig. S2 in ESI† and Table 2). This result is also in good agreement with literature, where it has already been reported, that reactive diluents have a positive effect on the curing behaviour of liquid isoprene rubber.24
Formulation | Conversion thiol groups (%) | Conversion vinyl groups (%) | Conversion main chain CC groups (%) |
---|---|---|---|
LIR-REF | — | — | 19 |
LIR-SH-TEG | 94 | 61 | 55 |
LIR-SH-DEG | 98 | 53 | 56 |
LIR-SH-BD | 51 | 72 | 65 |
Furthermore, FTIR data of the non-stabilized systems (Fig. S3 and Table S1 in ESI†) showed that pyrogallol influences the conversion of the functional groups. Without the addition of a stabilizer, dark reactions already proceed during the mixing of the resin formulation leading to a premature conversion of functional groups and a reduction of the remaining active moieties in the formulation. Thus, thiol and vinyl moieties are already partly consumed before the FTIR experiments have been carried out and a slowing down in the curing kinetics of the non-stabilized resin formulations is observed. In contrast, the addition of Sudan II to the stabilized resin formulations does not significantly affect the cure kinetics (Fig. S4 and Table S1 in ESI†).
However, the cure kinetics of all formulations reveals that the addition of the reactive diluents facilitates a high curing speed. In particular for stabilized systems, the polymerization process is nearly complete after 5 s of light exposure. At longer exposure times, the monomer conversion only slightly increases, which might be due to diffusion limitations of the rubber formulation at higher degree of conversion. Whilst LIR-SH-DEG and LIR-SH-TEG exhibit similar cure kinetics, LIR-SH-BD is characterized by a lower reactivity. Typically, we would expect that reactive diluents with shorter length of the glycol chains show an increased reactivity. However, the opposite behaviour was observed. These results are also corroborated by the photo-DSC data showing the highest photo-reactivity for tri(ethylene glycol) divinylether (LIR-SH-TEG), followed by di(ethylene glycol)divinylether (LIR-SH-DEG) and butandiol divinylether (LIR-SH-BD) as reactive diluents. Previous studies reported an increase in reaction rate for methacrylates with different pendant glycol chains.34 The higher reactivity was attributed to the mobility of the functional groups, which increases with rising spacer length and makes the functional groups better accessible during the reaction.
In addition, nearly full thiol conversion is observed in LIR-SH-DEG and LIR-SH-TEG, whilst the thiol conversion amounts to 51% in LIR-SH-BD. The results suggest that butandiol divinylether is more prone to side reactions than the other two divinyl ethers. In contrast to cationic photopolymerization, the electron-rich carbon double bonds of divinyl ethers do not undergo homopolymerization in photo-initiated radical polymerizations. However, it has been reported that co-polymerization with other alkenes is highly favoured.37 Thus, it is assumed that the carbon double bonds of butandiol divinylether in LIR-SH-BD preferably undergo a co-polymerization with the main chain CC double bonds of the rubber instead of participating in thiol–ene click chemistry.
The stress–strain behaviour of the photo-cured rubber formulations is displayed in Fig. 4 and the data are summarized in Table 3. The Young's modulus was calculated from the slope of the linear portion of the stress–strain curve. It should be noted that test specimens from LIR-REF were very weak and could not be removed from the moulds without destroying the samples. Therefore, no values could be obtained from LIR-REF. The poor mechanical properties are mainly related to the low reactivity of the resin formulation, which is associated with a low number of crosslinks.
Formulation | Stress (MPa) | Strain (%) | Young's modulus (MPa) |
---|---|---|---|
LIR-SH-TEG | 0.90 ± 0.12 | 42 ± 2 | 2.06 ± 0.42 |
LIR-SH-DEG | 0.78 ± 0.08 | 54 ± 3 | 1.45 ± 0.28 |
LIR-SH-BD | 0.32 ± 0.02 | 42 ± 3 | 0.78 ± 0.12 |
In contrast, adequate specimens were obtained with the rubber formulations containing the reactive diluents and as an example Fig. 5 illustrates the elasticity of LIR-SH-DEG by reversibly twisting the cured specimen by hand. In contrast to technical elastomers, the cured liquid rubber formulations show a rather low elongation at break. This is explained by the low molecular weight of the liquid rubber and the missing physical entanglements, which would significantly contribute to a rubber-like behaviour.
Fig. 5 Reversible twisting of a tensile test specimen from LIR-SH-DEG. The (a) initial test specimen was (b) twisted and could again be recovered to the (a) initial state. |
The highest stress and Young's modulus was found for LIR-SH-TEG indicating a higher rigidity compared to the other two systems. This behaviour is explained by the higher reactivity of TEG, which leads to higher crosslinked networks. Whilst photo-cured LIR-SH-DEG exhibits a similar behaviour, albeit at higher strain values, both stress and Young's modulus significantly decrease for photo-cured LIR-SH-BD. On the one hand, the low mechanical properties might be related to inhomogeneous network properties due to the high degree of co-polymerization and the associated decrease in crosslink density. On the other hand, photo-cured LIR-SH-BD contains a high amount of non-reacted thiols, which are well known to act as lubricants in thiol–ene networks.38
The non-stabilized rubber formulations showed poor results in the printing process. This was mainly due to the premature polymerization of the resin in the vat. Gelation occurred during the printing process, which led to either misshaped specimen or a complete stop of the layer-building. However, the addition of pyrogallol enabled the successful printing of well-defined structures. Specimens could be printed for LIR-SH-TEG and LIR-SH-DEG in a reasonable time.
However, due to the slower network formation of LIR-SH-BD the printing time had to be increased significantly. Fig. 6 displays the high resolution of the obtained specimen. The comb demonstrates very well the possible precision of the liquid rubber resins. All spikes (thickness decreases from 3 mm to 0.5 mm) were successfully printed and no accruing of the holes occurred. Thus, the results clearly showed that printing of liquid rubber formulations with bottom-up DLP techniques is feasible with a reasonable precision.
Fig. 6 DLP 3D printed specimen from LIR-SH-TEG: (a) comb and (b) gummy bear. (c) The precise structures of the printed gummy bear are shown in greater detail. |
Since the rubber formulations suffered from premature crosslinking reactions under dark conditions, 0.1 wt% of pyrogallol was added as stabilizer. Rheological measurements revealed that the stability of these rubber formulations was sufficiently high for the subsequent printing process.
Tensile tests revealed that the cured rubber networks suffer from a low strain (<100%) and stress (<1 MPa), which is mainly attributed to the low molecular weight of the liquid rubber and the absence of physical entanglements. In further work, strategies to improve the mechanical properties by network design and printing at higher temperature will be pursued.
However, the bottom-up DLP 3D printing of the rubber formulations could be successfully performed and 3D objects with adequate precision and good resolution were fabricated.
For the mixing, a two-axis centrifugal mixer “Vortex” from StateMix (Winnipeg, Canada) was employed. Due to the high viscosity of the liquid rubber it was not possible to dissolve the reactive diluents with a magnetic stirrer. Thus, all components, except the photoinitiators, were homogenized in one step by the Vortex mixer. Subsequently, the now low-viscous mixture was stirred on a magnetic stirrer at 50 °C to ensure a complete incorporation of the stabilizer. In a subsequent step, the photoinitiators were added and the mixture was stirred until all components dissolved into the formulation. The composition of the formulations is summarized in Table 4.
Sample | Type of reactive diluent | Concentration of reactive diluent/phr | Concentration of TMPMP/wt% | Molar ratio CC/thiol groups | Concentration of pyrogallol/wt% |
---|---|---|---|---|---|
LIR-REF | — | — | — | — | 0.1 |
LIR-SH-TEG | TEG | 30 | 44 | 1:1 | 0.1 |
LIR-SH-DEG | DEG | 30 | 57 | 1:1 | 0.1 |
LIR-SH-BD | BD | 30 | 64 | 1:1 | 0.1 |
For the photo-DSC measurements samples of 8 ± 0.05 mg were weighed in aluminium crucibles, which were analysed in a NETZSCH Photo-DSC 204 F1 Phoenix (Selb, Germany). The measurements were performed under nitrogen flow (20 mL min−1) at 50 °C. As light source an Omnicure s2000 UV-Lamp was used at 1 W cm−1.
FTIR measurements were performed on a VERTEX 70 (Bruker, Billerica, USA) in transmission mode to monitor the cure kinetics. 1 μL of the rubber formulation was placed on a Si-wafer and illuminated for a defined time with an Omnicure s1000 (Lumen Dynamics, Mississauga, USA) at 100% intensity (436 mW cm−2) with a 5 cm distance between sample surface and light source.
Tensile testing was performed according to ISO 37-S2 using a Z001 from Zwick Roell (Ulm, Germany) with a crosshead speed of 200 mm min−1. Measurements were carried out at room temperature. For sample preparation, silicon moulds with dimensions of 2 × 12.5 × 75 mm were prepared. The UV-curable rubber formulation was filled in the moulds and cured with a ND24 (Ostfildern, Germany) LED curing device at 385 nm for 10 min (124 mW cm−2). After curing, the samples were demoulded and washed with isopropanol.
The CAD drawings have been thankfully received from the Luxinergy GmbH (comb) and jakejake from http://thingiverse.com (gummy bear).
Footnote |
† Electronic supplementary information (ESI) available: FTIR spectra of LIR-REF and cure kinetics of stabilized and non-stabilized rubber formulations. See DOI: 10.1039/d0ra04186f |
This journal is © The Royal Society of Chemistry 2020 |