Sunmog Yeo*,
Won-Je Cho,
Dong-Seok Kim,
Chan Young Lee,
Yong Seok Hwang,
Jae Kwon Suk,
Chorong Kim and
Jun Mok Ha
Korea Multi-purpose Accelerator Complex, Korea Atomic Energy Research Institute, 38180, Republic of Korea. E-mail: sunmog@kaeri.re.kr
First published on 4th August 2020
H+ irradiation increases the surface hardness of polycarbonate. Nano indentation measurement shows that the hardness increases up to 3.7 GPa at the dose of 5 × 1016 # cm−2 and at the irradiation energy of 150 keV. In addition, the hardness increases with the dose and the energy of H+ irradiation. In accordance with the nano indentation measurement, the Fourier-transform infrared spectroscopy (FTIR) depends on the dose and energy of H+ irradiation. The peak at ∼1500 cm−1 for the aromatic ring and the peak at ∼1770 cm−1 for the CO stretch decrease with increasing dose and energy, while the increase of the dose and energy develops a new C
O stretch vibration at ∼1700 cm−1 and forms aromatic hydrocarbons at ∼1600 cm−1. X-ray diffraction experiments are also consistent with the nano indentation measurement and FTIR spectra. Based on the experiments, we discuss a possible mechanism of the surface hardness enhancements by ion beam irradiation.
On the other hands, polycarbonate (PC) has high heat resistance, optical clarity, dimension stability, and outstanding electrical resistance. Therefore, PC is known to be a versatile engineering polymer which is used in mechanical components, electric appliances, automotive industry, and so forth. However, PC is intrinsically soft and easily scratched, and thus, surface treatments are required before applying to the field which requires high surface hardness with inherent PC properties such as in vehicle light-weighting and optical sensors.15 There are varied surface treatments for PC. These include coating, ultra-violet irradiation and ion beam irradiation. Among these, ion beam irradiation has certain advantages; it is environmentally friendly and improves surface hardness and wear resistance. There have been several papers on the surface hardness enhancement of PC through ion beam irradiation.4–6 However, the enhancement mechanism of the surface hardness remains unclear. Some of the research simply alludes to crosslinking or the formation of carboxyl groups. In order to better understand the mechanism, more systematic studies are required. In this paper, the surface hardness and Fourier-transform infrared spectroscopy (FTIR) spectra for ion beam irradiated PC are examined with increasing dose and irradiation energy. Moreover, we explain the mechanism of the surface hardness enhancement by comparing FTIR spectra for H+ irradiated PC.
![]() | ||
Fig. 1 Surface hardness of H+ irradiated PC at the energy of 200 keV (red circles), 150 keV (blue triangles), and 100 keV (green squares). |
In order to scrutinize the energy dependence, a SRIM (Stopping and Range of Ion in Matter) calculation was performed for the H+ irradiated PC, as shown in Fig. 2(a). When energetically charged particles pass through matter, they lose their energy by colliding with electrons and nuclei in the matter. Before they come to stop, they collide more and more frequently with nuclei and form a damaged layer at a certain depth range. Fig. 2(a) shows the depth range of the damaged layers for 100 keV (green line), 150 keV (blue line), and 200 keV (red line). As expected, the higher energy generates the deeper damaged layer in matter.
![]() | ||
Fig. 2 (a) SRIM calculation results for the different irradiation energy and (b) load as a function of depth by sinus mode indentation test. |
The damaged layer can be detected by a nano-indentation test by using a sinus mode. Fig. 2(b) displays the indentation load versus indentation depth for the different irradiation energy. Of note is that, when the indentation depth increases, there is a kink of the load at a certain depth, which is indicative of the existence of the damaged layer by ion irradiation. In addition, the depth of the load kink increases with increasing irradiation energy, which is consistent with the SRIM calculation. However, the kink depth is less than the SRIM estimation. Since the nano-indentation measurement is affected by the below layer, the kink depth proceeds to the damaged layer. As the SRIM calculation shows that the full width at half maximum increases with increasing irradiation energy, the kink depth width also increases with increasing irradiation energy. It is notable that the kink depth widths for 100 keV, 150 keV, and 200 keV are 0.08 μm, 0.14 μm, and 0.19 μm, respectively. In addition, the load slope increases with increasing irradiation energy, meaning that the PC surface hardness increases with increasing irradiation energy. This analysis is consistent with the surface hardness shown in Fig. 1.
Fig. 3 shows the FTIR spectra of the original PC and H+ irradiated PC for different energy. For the irradiation energy of 100 keV, as shown in Fig. 3(a), the black, green, blue line, and red lines represent the FTIR spectrum of pristine PC, H+ irradiated PC with the dose of 1015 # cm−2, 1016 # cm−2, and 5 × 1016 # cm−2, respectively. The FTIR spectrum of the pristine PC has strong transmittance peaks at 1500 cm−1 and 1770 cm−1, which originated from the aromatic ring and CO stretching vibration, respectively. However, H+ irradiation systematically suppresses two peaks of pristine PC; the higher H+ dose makes the two peaks lower. Moreover, the higher H+ dose produces a new peak at ∼1700 cm−1 and develops a greater aromatic hydrocarbon peak at ∼1600 cm−1. The new peak at ∼1700 cm−1 can be identified as another C
O stretching vibration.16 In fact, the carbon in the C
O bonds of pristine PC also forms bonds with other oxygen: C–O single bonds. The FTIR transmittance peak at ∼1770 cm−1 reflects all these connections. When H+ ions are irradiated, however, C–O single bonds are easily broken, compared with C
O double bonds, because the bonding energy of C–O is lower than that of C
O. Although bonds are broken by certain actions, they try to recover or form bonds with neighboring atoms; the higher H+ dose leads to a greater chance of C–H single bond formation. In other words, a new C
O stretching vibration peak for the H+ irradiated PC can be developed at a low wavenumber in the FTIR spectra. Indeed, H+ irradiation on PC develops a new C
O stretching vibration around 1700 cm−1 and suppresses C
O stretching vibration around 1770 cm−1, as shown in Fig. 3(a). This mechanism also explains the FTIR spectra for the PC irradiated by 150 keV (shown in Fig. 3(b)) and 200 keV (not shown here). In Fig. 3(b), the black, green, blue, and red lines represent the FTIR spectra of pristine PC, and H+ irradiated PC with the dose of 1015 # cm−2, 1016 # cm−2, and 5 × 1016 # cm−2, respectively.
In addition, H+ irradiation can also lead to an aromatic hydrocarbon peak around 1600 cm−1 in the FTIR spectra. Since aromatic hydrocarbons have sigma bonds, the bonding energy of an aromatic hydrocarbon is larger than that of an aromatic ring. Therefore, the transmittance peaks of the aromatic hydrocarbons have higher wavenumbers than those of aromatic rings in the FTIR spectra. Again, H+ irradiation supplies more chances to form aromatic hydrocarbons by rearranging the bonds of aromatic rings. Fig. 3(a) shows that the higher H+ irradiation dose causes the higher peaks for aromatic hydrocarbons and the lower peaks for aromatic rings at the energy of 100 keV. The same mechanism can be also applied to the FTIR spectra for the other energies such as 150 keV (shown in Fig. 3(b)) and 200 keV (not shown here).
The surface hardness of H+ irradiated PC has energy dependence where the surface hardness increases with increasing irradiation energy. In order to certify the energy dependence, FTIR spectra were obtained from the H+ irradiated PC with different energy at the dose of 5 × 1016 # cm−2, as shown in Fig. 4. The black, green, blue, and red lines represent the FTIR spectra of pristine PC, and H+ irradiated PC with the energies of 100 keV, 150 keV, and 200 keV, respectively. Interestingly, by increasing the H+ irradiation energy, the transmittance peaks for CO stretching vibration around 1770 cm−1 and aromatic ring decrease while the transmittance peaks for C
O stretching vibration around 1700 cm−1 and aromatic hydrocarbons are developed. In conjunction with the surface hardness shown in Fig. 1, the FTIR spectra change very systematically with increasing H+ irradiation dose and energy, as shown in Fig. 3 and 4. This means that surface hardness enhancement is related to the development of the new C
O stretching vibration around 1700 cm−1 and aromatic hydrocarbons formation. In other words, H+ irradiation produces a new C
O stretching vibration around 1700 cm−1 and forms more aromatic hydrocarbons, which is a reason for the hardness enhancement of H+ irradiated PC.
Fig. 5 shows the X-ray data of pristine PC and H+ irradiated PC. The black, the green, the blue, and the red lines are the X-ray data of pristine PC and H+ irradiated PC with the energies of 100 keV, 150 keV, and 200 keV, respectively. In order to compare energy dependency, the X-ray data were obtained from the same dose of 1016 # cm−2. It is known that X-ray diffraction for amorphous PC has a broad peak at 2θ = ∼17°,17 which is the same as pristine PC. Interestingly, the X-ray data for H+ irradiated PC show two peaks at low angles. This indicates that H+ irradiation changes the properties of PC through crosslinking and forming new CO stretch bonds and aromatic hydrocarbons. Moreover, the broad peak intensity decrease with increasing the H+ irradiation energy, suggesting that H+ irradiation leads to the amorphous behaviour of pristine PC to become weak. Generally speaking, an amorphous state is softer than a crystal state, and thus, the X-ray behaviour is consistent with the surface hardness and FTIR spectra.
![]() | ||
Fig. 5 X-ray diffraction data for pristine PC and H+ irradiated PC with the energy of 100 keV, 150 keV, and 200 keV. |
When energetic particles with the energy of 100 keV pass through polymers, they can break all the neighboring bonds whose energy are at most 10 eV. The broken bonds in a polymer chain can form bonds in other polymer chains, meaning that crosslinks occur by ion beam irradiation. In fact, it is known that crosslinks are a general reason to increase surface hardness. In this experiment, H+ irradiation also produces crosslinks between polymer chains in PC. In addition to crosslinks, H+ irradiation also generates new CO stretch bonds and aromatic hydrocarbons. Consequently, the surface hardness enhancement by H+ irradiation results from all these effects.
This journal is © The Royal Society of Chemistry 2020 |