Cristopeer Thomas-Busania,
José Andrei Sarabia-Sainzb,
Jaqueline García-Hernándezc,
Tomás J. Madera-Santanad,
Luz Vázquez-Morenoa and
Gabriela Ramos-Clamont Montfort*a
aCoordinación de Ciencia de los Alimentos, Centro de Investigación en Alimentación y Desarrollo A.C., Carretera Gustavo Enrique Astiazarán Rosas, No. 46. Col. La Victoria, C.P. 83304, Hermosillo, Sonora, Mexico. E-mail: gramos@ciad.mx
bLaboratorio de Biofísica Médica, Departamento de Investigación en Física, Universidad de Sonora, Blvd. Luis Encinas y Rosales. Col. Centro, C.P. 83000, Hermosillo, Sonora, Mexico
cCoordinación Guaymas, Centro de Investigación en Alimentación y Desarrollo, Sánchez Taboada Carretera al Varadero Nacional km 6.6, Col. Las Playitas, Guaymas, Sector Varadero, Las Playitas, 85480 Heroica Guaymas, Son, Mexico
dCoordinación de Tecnología de Alimentos de Origen Vegetal, Centro de Investigación en Alimentación y Desarrollo, Carretera Gustavo Enrique Astiazarán Rosas, No. 46. Col. La Victoria, C.P. 83304, Hermosillo, Sonora, Mexico
First published on 3rd August 2020
The uptake of arsenite [As(III)] and arsenate [As(V)] by functionalized calcium alginate (Ca-Alg) beads from aqueous solutions was investigated. Ca-Alg beads were protonated with poly-L-lysine (PLL) or polyethyleneimine (PEI) using 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide/N-hydroxysuccinimide (EDC/NHS) or glutaraldehyde (GA) as crosslinking agents. Four types of protonated beads were prepared: Ca-Alg-EDC/NHS (PLL or PEI) and Ca-Alg-GA (PLL or PEI). Fourier transform infrared spectroscopy in total attenuated reflection mode (FTIR-ATR), analysis showed presence and increased intensity of bands corresponding to OH, NH, CH2 and CH3 groups in modifications with both polycations. In addition, thermogravimetric analysis and atomic force microscopy of all modified capsules showed an increase in thermal stability and uniformity of the capsules, respectively. Ca-Alg-EDC/NHS-PLL beads had the maximum adsorption capacity of [As(V)] (312.9 ± 4.7 μg g−1 of the alginate) at pH 7.0 and 15 minute exposure, while Ca-Alg-EDC/NHS-PEI beads had the maximum adsorption capacity of [As(III)] (1052.1 ± 4.6 μg g−1 of alginate). However, all these EDC containing beads were degraded in the presence of citrate. Ca-Alg-GA-PEI beads removed 252.8 ± 9.7 μg of [As(V)] μg g−1 of alginate and 524.7 ± 5.3 de [As(III)] μg g−1 of alginate, resulting the most stable capsules and suitable for As removal.
Arsenic leaches into water bodies from natural deposits or waste generated by anthropogenic activities. The last include mining and metallurgy, industries producing paint and wood preservatives, and the application of persistent arsenic fertilizers (currently prohibited).4 The most common As chemical forms in water are arsenate [As(V)] and arsenite [As(III)]. The latter is more toxic, water-soluble, abundant, and difficult to remove.2 Biosorption using alginate represents an alternative to removing low concentrations of As (10–100 μg L−1) from drinking water.5
Alginate has been shown to be a good adsorbent of heavy metals. This anionic polymer, typically extracted from brown seaweed, is cheap to produce and generally recognized as safe (GRAS).6 The crosslinking of alginate with divalent ions such as Ca2+ allows the formation of hydrogels with a structure called egg-box. The hydrogel can be synthesized in the form of capsules using the extrusion dripping method.7 Nussinovitch and Dagan (ref. 8) used alginate–gellan capsules to remove several heavy ions from solutions and showed high adsorption efficiencies to Pb2+, Cu2+, Cd2+, and Ni2+. (316, 219, 197, and 65 mg g−1 of dry alginate, respectively). Calcium alginate beads have also been successfully used to remove Ag2+, Au2+, Cd2+, and Cu2+ ions.9 In these studies, the biosorption mechanism is based on conventional charge interactions, that is the cation's affinity to negative charged alginate.9 This mechanism could not be used for biosorption of [As(III)] and [As(V)] because these ions carry total negative charges. However, an additional advantage of alginate is that the surface of its capsules can be functionalized to acquire new properties and allow new interactions to be established.10
The protonation of alginate with polycations is possible due to the stability of alginate negative charge over a wide pH range.5 This feature allows the formation of complexes with strongly positively charged moiety like ions present in poly-L-lysine (PLL), poly-L-ornithine (PLO), poly-methylene-co-guanidine (PMCG), polyethyleneimine (PEI) and chitosan.11 Formation of positively charged alginate beads comes from electrostatic interactions established between positive polycation groups and alginate carboxyl groups on the outer layer of alginate capsules. These positive particles are more stable, less porous and more biocompatible with the human organism. Thus, they are studied in biomedical applications such as controlled drug release, organ transplantation and tissue engineering.12,13 The downfall of these positively charged beads is that they can be destabilized by changes in pH or ionic strength.11
One way to form more stable alginate protonated beads is by the conjugation of polycations with alginate using a crosslinker, for example, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide (EDC) or glutaraldehyde (GA). These interconnecting agents have been tested in tissue engineering by crisscrossing them with collagen.9 Poly-L-lysine (PLL) and polyethyleneimine (PEI) are good candidates for the formation of alginate–polyanion gels due to their low cost and high availability.14 Alginate–polyethylene network formed using GA as a crosslinker increased the stability of alginate capsules loaded with different microorganisms.11 EDC supported crosslinked alginate with different molecules has been investigated as copper ion removal network, controlled drug release capsules, and tissue engineering scaffolds.15,16 The common strategy to synthesize alginate protonated gels is to prepare suspensions of alginate, mix them with the polyanion to start crosslinking reaction and finally add the crosslinking.11,15,16
To properly design alginate–polyanion gel beads for [As(V)] and [As(III)] adsorption, the amino groups of PLL and PEI need to be exposed on the surface of the capsules. The crosslinker EDC reacts with the carboxyl groups of the alginate forming an unstable intermediate. The addition of N-hydroxysuccinimide (NHS) stabilizes the system by forming an ester. When the polycations are added to alginate beads, a nucleophilic substitution of type SN2 is carried out, where the ester is replaced by the amino groups present in the polycations, allowing the formation of a covalent amide-type bond, between the amino groups of polycations and carboxyl groups (mannuronic acid blocks that do not intervene in calcium gelling) of alginate.9 Fig. 1A represents a model of this reaction when using PLL or PEI.
Fig. 1B shows a model of crosslinking reaction using glutaraldehyde (GA). By submerging alginate capsules into polycation solutions, there are electrostatic interactions with the alginate carboxyl groups, which are unstable. The role of GA is to stabilize such interactions as it can react with both the amino groups of polycations and with the hydroxyl groups of the alginate.17 This crosslinking prevents polycations from dissociating due to changes in pH or ion strength, by forming covalent bonds of acetal type with hydroxyl and imine bond with amines.11
Therefore, we propose to obtain first the capsules of calcium crosslinked alginate and then treat them with the polycations in the presence of the crosslinkers. After characterization, they were used as bio-sorbent matrices for [As(III)] and [As(V)] in aqueous solution.
When GA was used as crosslinker, the Ca-Alg beads were first immersed, separately, in 200 mL of PEI solution at 1.5% (w/v) or PLL at 1.5% (v/v) for 24 h at 25 °C. Then, they were collected and immersed in 100 mL of 2% (v/v) GA solution for 1 h. The modified beads were collected, washed three times with deionized water to remove unreacted PEI, PLL, and GA. These samples were labelled as Ca-Alg-GA-PLL and Ca-Alg-GA-PEI.
Beads surface charge was determined at 25 °C by measuring their zeta potential (ζ), in a Zetasizer Nano-ZS90 (Malvern Instrument Ltd. Worcestershire, UK). Beads were suspended in deionized water. To assay the effect of the pH of normal drinking water over protonated alginate, ζ of the capsules was determined in a range of 6.0 to 7.5. Measurements were made in triplicate, with 100 runs per replicate. The pH was adjusted with 1 M NaOH and 1 M HCl solutions.
The removal efficiency was calculated using the following equation:
ER = (Ci − Cf)100/Ci |
The maximum adsorption capacity was calculated using the following equation:
Qe = (C0 − Ce)V/m |
Treatment | Size (mm) | Moisture content (%) | Z potential (mV) |
---|---|---|---|
a Ca-Alg: calcium alginate beads. Crosslinking agents EDC/NHS: 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide/N-hydroxysuccinimide; GA: glutaraldehyde. Values are expressed as means ± standard error. Different letters in the same column denote a statistical difference (p < 0.05). | |||
Ca-Alg (control) | 1.27 ± 0.09a | 96.14 ± 0.4a | −27.5 ± 1.46a |
Ca-Alg-EDC/NHS-PLL | 1.27 ± 0.13a | 92.92 ± 0.13b | +23.6 ± 0.15c |
Ca-Alg-EDC/NHS-PEI | 1.26 ± 0.19a | 93.32 ± 0.05b | +23.3 ± 0.27c |
Ca-Alg-GA-PLL | 1.23 ± 0.11b | 90.26 ± 0.63c | +0.64 ± 0.12d |
Ca-Alg-GA-PEI | 1.20 ± 0.11c | 82.14 ± 1.04d | +10.3 ± 0.16e |
The GA crosslinked beads (Ca-Alg-GA-PLL and Ca-Alg-GA-PEI) were oval shape (Fig. 2D and E). Also, smaller in size and moisture content (p < 0.05) than Ca-Alg capsules (Table 1). When reacting with GA, alginate loses OH groups that can otherwise be available to capture water through the formation of hydrogen bonds.9 In addition, during the reaction of the amine from polycation (nucleophilic) with the carbonyl (electrophile) of the GA, a hemiaminal intermediary (NH-CR2-OH) is formed, followed by the loss of water during the formation of the imine bond (CN). These processes produce slight dehydration of the capsules.19,20 The surface charge of the Ca-Alg-PLL-GA and Ca-Alg-PEI-GA beads had positive values (+0.6273 ± 0.12 mV and +10.29 ± 0.16, respectively). Furthermore, the positive surface charge was greater (P < 0.05) when using EDC/NHS than GA as a crosslinker (Table 1). This may be due to the type of cross-connection formed, as carbodiimide increases amines exposure to the polycation.
In contrast to EDC/NHS formed capsules, both types of GA hardened capsules were opaque. In addition, Ca-Alg-GA-PEI capsules gained a red color (Fig. 2E). The red color is an indication of the formation of unsaturated alternating imine-type bonds resulting from the reaction between GA and PEI.21 The lack of red color in Ca-Alg-GA-PLL capsules is possibly due to a lower degree of crosslinking between PLL and GA than between PEI and GA since PLL molecule has fewer amino groups than PEI molecule.9
The pH changes, within the studied range (6.0–7.5), had no effect (p > 0.05) on the surface charge of any of the modified capsules, PEI nor PLL (data not shown). This stability confirms that both the PEI amino groups, as well as those of PLL, remained protonated at the pH commonly found in drinking water.22
Fig. 3 Attenuated total reflectance Fourier transform infrared spectroscopy for calcium alginate beads functionalized with (A) poly-L-lysine and (B) polyethylenimine. |
The crosslinking of the alginate with PLL using EDC/NHS modified the bands corresponding to the stretching of the OH groups of the alginate at 3334 cm−1 (Fig. 3A). An increase in peak intensity and the appearance of two small, new bands at 3348 cm−1 and 3237 cm−1 coincide with amide A region thus indicating the formation of amide-type covalent bonds between the amino groups of the PLL and the carboxyl groups of alginate.9 The signal corresponding to the COO-asymmetrical groups in the Ca-Alg capsules (1593 cm−1) appeared as a higher intensity band in the Alg-EDC/NHS-PLL capsules. In addition, there was a slight displacement to 1608 cm−1 possibly due to the interactions between the carbonyl of alginate and the amine of PLL. These changes are indications of the interaction of the COO-groups of the alginate with the NH2 groups of the PLL.14
The crosslinking with PLL using GA showed as an increase in the intensities of the bands corresponding to the methylene groups, attributed to the presence of these groups in the lateral chains of the PLL incorporated on the surface of the alginate beads. In addition, the appearance of a small band at 1697 cm−1 was observed that can be attributed to the bending of the amino groups present in the PLL attached to the alginate matrix. The band at 822 cm−1 shifted to 805 cm−1 which is an indication of the incorporation of the PLL to the alginate.23
The crosslinking of alginate with PEI using EDC/NHS was characterized by a broad band at 3148 cm−1, attributed to the OH groups of alginate and NH of PEI (Fig. 3B). Besides, two small bands appeared at 3341 and 3267 cm−1, assigned to the PEI amino groups attached to the alginate matrix. The peaks at 2911 and 2807 cm−1 corresponding to C–H stretch of CH2 and CH3 groups significantly increased their intensity due to the incorporation of PEI methylene groups at the surface of alginate capsules.24 The signal corresponding to the COO-asymmetrical bend in the Ca-Alg capsules (1593 cm−1) shifted to 1585 cm−1, due to interactions with the amino groups of the PEI. The band at 1029 cm−1, (C–O–C and/or C–N), also showed a slight displacement (1022 cm−1). The band at 881 cm−1 which corresponds to the signal of the primary amines, proves the amine group presence into the alginate capsules.23
In the spectra of Ca-Alg-PEI capsules crosslinked with GA, an increase in the intensity of the OH group band (3274 cm−1) is well visible due to the presence of NH groups from PEI. Unlike in crosslinking with EDC/NHS, bands in 3341 and 3267 cm−1 did not appear, because covalent links between alginate and PEI are not formed in the same manner. However, the intensity of the peak at 2933 cm−1 increased and a band at 2837 cm−1 appeared due to additional CH2 and CH3 groups from the PEI polymer. The peak at 1593 cm−1 shifted to 1585 cm−1 attributed to the formation of imine bonds between GA aldehyde and PEI amine group, confirming covalent bonding of the polycation coating to the alginate matrix.24 The measured wavenumbers of the bands before and after the modification are summarized in Table 2.
Ca-Alg | Ca-Alg-EDC/NHS | Ca-Alg-GA | Assignment | ||
---|---|---|---|---|---|
PLL | PEI | PLL | PEI | ||
a Ca-Alg: calcium alginate beads. Crosslinking agents EDC/NHS: 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide/N-hydroxysuccinimide; GA: glutaraldehyde. ν: stretching; a: asymmetric; s: symmetric. | |||||
3300 | 3334 | 3148 | 3274 | 3274 | ν(OH) |
— | 3348; 3237 | 3341; 3267 | 3274 | 3274 | ν(N–H) |
2933 | 2933 | 2911; 2807 | 2949 | 2933; 2837 | ν(C–H) |
— | 1697 | ν(N–H) | |||
1593 | 1618 | 1585 | 1585 | νa(COO−) | |
1415 | 1415 | 1415 | 1415 | 1415 | νs(COO−) |
1029 | 1029 | 1022 | 1029 | 1022 | ν(C–O–C) |
— | 822 | 881 | 805 | 881 | ν(N–H) |
The thermogram of the Ca-Alg-EDC/NHS-PLL capsules showed a degradation process in two stages. The first stage began at 33 °C and ended at 107 °C, with a maximum degradation occurring at 84 °C. This step represents moisture loss and degradation of alginate. The second degradation occurred between 199 °C and 496 °C, with a maximum degradation at 201 °C. This degradation can be attributed to the decomposition of the polyamine acid. Similar patterns of lysine and arginine decomposition was reported by Zhang et al.22 Ca-Alg-PEI capsules crosslinked with GA showed a one-step degradation starting at 49 °C and ending at 182 °C, with a maximum degradation at 168 °C. This increase in the thermal stability of alginate beads is due to the matrix and polycation interactions forming a harder network. Similar behaviour was reported by Poon et al.20 in chitosan copolymers.
Fig. 5 shows the thermograph curves of PEI-modified alginate capsules (A) and their derivatives (B). The thermograph of Ca-Alg-EDC/NHS-PEI capsules had a one-stage decomposition, similar to Ca-Alg capsules. However, the initial degradation and maximum degradation temperatures increased from 33 °C to 46 °C and from 111 °C to 153 °C, respectively. These thermal shifts indicate greater thermal stability of the capsules due to formations of a stable crosslinked network between the alginate matrix and the PEI groups.26
Crosslinking PEI using GA presented changes in its decomposition pattern again showing thermal degradation in several stages. The first, between 43 °C and 195 °C, with a maximum degradation at 128 °C can be attributed to the loss of moisture and thermal degradation of alginate.
The second degradation occurred between 198 °C and 368 °C, with a maximum decomposition at 205 °C can be assigned to the breakdown of glutaraldehyde, which occurs very quickly.27 The final stage occurs between 361 °C and 496 °C and can be recognized as the degradation of PEI, with a maximum degradation at 377 °C.17 Overall, the thermographs of the modified alginate capsules with PLL or PEI, using EDC/NHS or GA as crosslinkers showed an improvement in thermal stability, compared to uncross linked Ca-Alg capsules. This improvement in thermal stability can be explained by the decrease in the mobility of the alginate molecules due to their connection to polycation PLL or PEI. Also, the presence of polycations protects the surface of the capsules exposed to heat and decreases mass loss during thermal decomposition of the sample.26
Formulation | As(V) | As(III) | ||
---|---|---|---|---|
Removal efficiency (%) | Biosorption capacity (μg g−1) | Removal efficiency (%) | Biosorption capacity (μg g−1) | |
a Ca-Alg: calcium alginate beads. Crosslinking agents EDC/NHS: 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide/N-hydroxysuccinimide; GA: glutaraldehyde. Values are expressed as means ± standard error. Different letters in the same column denote a statistical difference (p < 0.05). | ||||
Ca-Alg (control) | 0.38 ± 0.0d | 11.7 ± 1.1d | 0.8 ± 0.1e | 21.3 ± 1.7d |
Ca-Alg-EDC/NHS-PLL | 17.3 ± 0.1b | 312.9 ± 4.7a | 25.2 ± 0.4d | 448.5 ± 5.6c |
Ca-Alg-EDC/NHS-PEI | 14.0 ± 0.6c | 249.6 ± 12.2b | 58.9 ± 0.4b | 1052.1 ± 4.6a |
Ca-Alg-GA-PLL | 12.2 ± 0.4c | 152.6 ± 0.6c | 36.7 ± 0.3c | 458.4 ± 4.3c |
Ca-Alg-GA-PEI | 37.9 ± 1.0a | 252.8 ± 9.7b | 69.9 ± 0.7a | 524.7 ± 5.3b |
Ca-Alg-GA-PEI beads were also most efficient (69.9 ± 0.7%) in arsenite adsorption (Table 3), while Ca-Alg-EDC/NHS-PEI capsules showed the maximum adsorption per g capacity of dry alginate (1052.1 ± 4.6 μg g−1 of dry alginate). At pH 7.0 the predominant species of [As(III)] is arsenous acid (H3AsO3), which is neutral in a wide range of pH (from 2 to 9.2).31 It has been suggested that the main adsorption mechanism for this form of arsenic species is chelation of [As(III)] ions by the functional groups of the adsorbent. The [As(III)] behaves like a Lewis acid with an incomplete octet and is able to capture free electrons. On the other hand, the amino groups present of the alginate–polycation capsules, behave like Lewis bases, donating free electrons, forming the chelate complexes via one of the two-bonded ligands.33
Most treatments designed to remove As from water focus on the removal of [As(V)] but fail or ignore to eliminate [As(III)]. One of the strategies for the elimination of [As(III)] is to oxidize it to [As(V)] using pre-treatment with chlorine or permanganate. During As adsorption, a non-redox-sensitive sorbent such as MnO2 can also be used to transform [As(III)] into [As(V)] without requiring pretreatment.34 However, some substances present in water may interfere with this oxidation.5 Shakoor et al.35 studied several biosensors for the removal of [As(III)] and [As(V)] at pH of 7.0. They found that eggshells and plum pits were able to remove 85% and 67% of the [As(III)] respectively after 2 hours of contact. However, the pH had to be reduced to 4.5 in order to adsorb [As(V)]. CuO-functionalized graphene/carbon NTs (CuO-CNTs) were able to remove 2.3 mg g−1 of [As(III)] and 2.4 mg g−1 of [As(V)] at pH of 7 and 5, respectively (contact times of 60 min and 40 min, respectively).36 Although the alginate–polyanion capsules synthesized in this study showed lower adsorption capabilities (Table 3), have the advantage of removing an acceptable amount of [As(III)] and [As(V)] in short contact times and without pH modification.
Fig. 7 EDX in SEM images of (A) calcium alginate beads; (B) Ca-Alg-GA-PEI beads; (C) Ca-Alg-GA-PEI beads after biosorption of [As(III)]; (D) Ca-Alg-GA-PEI beads after biosorption of [As(V)]. |
Fig. 8 Attenuated total reflectance Fourier transform infrared spectroscopy for Ca-Alg-GA-PEI beads before and after [As(III)] or [As(V)] adsorption. |
In groundwater inorganic oxyanions such as trivalent arsenite [As(III)] and pentavalent arsenate [As(V)] are the predominant As species.5 In this aqueous environment the adsorption of [As(III)] and [As(V)] is mainly governed by the pH because it regulates the ionic characteristics of both species as wells as the surface properties of the sorption matrix. At pH 7 [As(III)] is mostly in its neutral form (H3AsO3 = H2AsO3− + H+, pKa1 = 9.2) and approximately 50% of amino groups remain unprotonated.5,37–39 In this context [As(III)] uptake by Ca-Alg-GA-PEI beads is determined by surface complexation of H3AsO3 with NH2 groups.37 This is in agreement with the observations of Daikopoulos et al.39 who synthetized amine-rich graphitic carbon nitride for arsenite remediation.
Arsenite biosorption capacity of Ca-Alg-EDC/NHS-PEI beads was higher (1052.1 ± 4.6 μg g−1) than that of Ca-Alg-GA-PEI ones (524.7 ± 5.3 μg g−1) (Table 3). The crosslinker EDC reacts with the carboxyl groups of the alginate forming an unstable intermediate (Fig. 1). The addition of N-hydroxysuccinimide (NHS) stabilizes the system by forming an ester, then the ester is replaced by the amino groups present PEI, allowing the formation of a covalent amide-type bond, between the amino groups of polycations and carboxyl groups (mannuronic acid blocks that do not intervene in calcium gelling) of alginate.9 On the contrary GA reacts with the amino groups of PEI and the hydroxyl groups of the alginate.17
This type of reaction allows a greater crosslinking between the alginate and PEI both on the bead surface and within the supporting alginate matrix forming a 3D network that increase the bead stability but also the [As(III)] binding sites with the free amino groups that did not react with GA.40 Then excessive crosslinking can adversely affect the binding capacity of the matrix as it seems to have happened with Ca-Alg-GA-PEI. Subsequent experiments should be conducted testing different concentrations of GA in order to find a more adequate balance between crosslinking and available binding sites.
Ca-Alg-EDC/NHS-PLL and Ca-Alg-GA-PLL presented lower biosorption capacities for [As(III)] (p < 0.05) than the matrices cross-linked with PEI. This may be because PLL has fewer amino groups than PEI and therefore fewer junction points for arsenite. The biosorption capacities of both (Ca-Alg-EDC/NHS-PLL and Ca-Alg-GA-PLL) were similar to each other (448.5 ± 5.6 μg g−1 and 458.4 ± 4.3 μg g−1, respectively), which is an indication of a lower crosslinking of PLL with GA. This can be seen with the naked eye by comparing the colors of Ca-Alg-GA-PLL (opaque white) and Ca-Alg-GA-PEI (reddish orange) (Fig. 2). The reaction between GA and amines produces compounds with yellow to orange colorations.21 Both Ca-Alg-EDC/NHS-PLL and Ca-Alg-GA-PLL showed low stability, so more research should be done on how to improve them.
At pH 7.0 about half of the surface amino groups are protonated and H2AsO4− and HAsO42− are predicted to appear.5,38 Under such a condition, [As(V)] is readily retained by the Ca-Alg-GA-PEI beads via electrostatic interaction. Fig. 9 presents the interactions of oxyanions of [As(III)] and [As(V)] with PEI amine groups.
Fig. 9 Schematic representation of the complex interactions of [As(III)] and electrostatic interaction of [As(V)] with Ca-Alg-GA-PEI amine groups. |
Ca-Alg-EDC/NHS-PLL showed higher [As(V)] adsorption capacity compared to the other matrices (Table 3), this correlates with its net surface charge of +23.6 ± 0.15 mV (Table 1). Ca-Alg-EDC/NHS-PEI showed similar values of net surface charge but lower biosorption capacity than Ca-Alg-EDC/NHS-PLL. This results may be due to the cross-linking of the amino groups with GA. Ca-Alg-GA-PEI showed an [As(V)] uptake similar to Ca-Alg-EDC/NHS-PEI (252.8 ± 9.7 μg g−1 and 249.6 ± 12.2 μg g−1, respectively), despite the fact that Ca-Alg-GA-PEI showed a surface charge of +10.3 ± 0.16 mV (Table 1). This may indicate that [As(V)] was retained not only in the surface but also within the supporting bead matrix. This is possible due to the ability of GA to react with the OH groups of the alginate and the amino groups of PEI or PLL and also explains why the Ca-Alg-GA-PLL beds were able to capture [As(V)] even though they showed a surface charge of +0.64 ± 0.12 mV (Table 3).
A very nominal decrease in [As(III)] and [As(V)] removal capacity in five consecutive cycles of sorption/adsorption demonstrates the reusability of Ca-Alg-GA-PEI (Fig. 10). A 9% of arsenate decrease was observed until the fifth sorption/adsorption cycle.
Fig. 10 Removal efficiency of Ca-Alg-GA-PEI after five desorption/adsorption cycles. Asterisk denotes significant difference (p < 0.05) between the cycles of the same oxyanion. |
Arsenic adsorption strongly depends of water pH. The range of effective adsorption of both [As(III)] (H2AsO3) and [As(V)] (H2AsO4− and HAsO42−) occurs between a water pH of 6.0 to 7.5. More acidic conditions will increase the adsorption of [As(V)] while more alkaline conditions will increase the adsorption of [As(III)].5 At pH of 7.0, Ca-Alg-GA-PEI beads adsorbed both [As(III)] and [As(V)]. This could represent an advantage for water treatment. However, subsequent isotherms, kinetics and thermodynamic studies must be conducted in order to establish the matrix behavior at different pH, redox potential and different sorbent, sorbate and arsenic oxyanions concentrations. Such studies will provide more accurate information aimed at improving the optimal conditions of use for Ca-Alg-GA-PEI for As removal at specific conditions.
This journal is © The Royal Society of Chemistry 2020 |